Article(id=1188049578868748895, tenantId=1146029695717560320, journalId=1185652524569653253, issueId=1188049574255018819, articleNumber=1009-5438(2024)01-0020-04, orderNo=null, doi=null, pmid=null, cstr=null, oa=null, hot=null, price=null, onlineType=0, articleFormat=0, articleType=null, articleTypeStr=null, receivedDate=1703692800000, receivedDateStr=2023-12-28, revisedDate=null, revisedDateStr=null, acceptedDate=null, acceptedDateStr=null, onlineDate=1761182692496, onlineDateStr=2025-10-23, pubDate=1708790400000, pubDateStr=2024-02-25, doiRegisterDate=null, doiRegisterDateStr=null, onlineIssueDate=1761182692496, onlineIssueDateStr=2025-10-23, onlineJustAcceptDate=null, onlineJustAcceptDateStr=null, onlineFirstDate=null, onlineFirstDateStr=null, sourceXml=null, magXml=null, createTime=1761182692496, creator=13701087609, updateTime=1761182692496, updator=13701087609, issue=Issue{id=1188049574255018819, tenantId=1146029695717560320, journalId=1185652524569653253, year='2024', volume='50', issue='1', pageStart='1', pageEnd='98', issueExtLink='null', onlineDate='null', pubDate='null', beforeIssueId=null, nextIssueId=null, price=null, status=1, issueComplete=1, articleOrder=1, issueType=-1, specialIssue=null, createTime=1761182691396, creator=13701087609, updateTime=1761290996781, updator=13701087609, preIssue=null, nextIssue=null, ext={EN=IssueExt(id=1188503840023265810, tenantId=1146029695717560320, journalId=1185652524569653253, issueId=1188049574255018819, language=EN, specialIssueTitle=, coverIllustrator=null, specialIssueEditor=, specialIssueAbout=), CN=IssueExt(id=1188503840023265811, tenantId=1146029695717560320, journalId=1185652524569653253, issueId=1188049574255018819, language=CN, specialIssueTitle=, coverIllustrator=null, specialIssueEditor=, specialIssueAbout=)}, issueFiles=null}, startPage=20, endPage=23, ext={EN=ArticleExt(id=1188049579049103969, articleId=1188049578868748895, tenantId=1146029695717560320, journalId=1185652524569653253, language=EN, title=Analysis and Treatment for Temperature Increase of Hearth Side Wall of 7
# Blast Furnace of Baotou Steel, columnId=1187100781414069182, journalTitle=Science & Technology of Baotou Steel, columnName=Production Practices and Management, runingTitle=null, highlight=null, articleAbstract=
In this paper, it is analyzed the causes of abnormal temperature increase of side wall at tap hole for hearth of 7# blast furnace of Baotou Steel and emphasized the treatment measures. With the long-term high-intensity smelting conditions, tap hole of hearth is relatively active and its length is controlled poorly so that scour of slag iron to carbon brick of tap hole is aggravated. As a result, the erosion of carbon brick of tap hole is the cause for temperature increase of side wall at tap hole for hearth of 7# blast furnace. The temperature of side wall at tap hole is effectively controlled without reducing the smelting intensity and output of 7# blast furnace through taking such measures as increasing the quantity of circulating water at tap hole to improve cooling intensity, carefully maintaining tap hole, actively eliminating air gap of hearth side wall as well as appropriately opening central gas stream and restraining gas stream at edge for the charging system.
, correspAuthors=null, authorNote=null, correspAuthorsNote=null, copyrightStatement=null, copyrightOwner=null, extLink=null, articleAbsUrl=null, sourceXml=null, magXml=null, pdfUrl=null, pdf=null, pdfFileSize=null, pdfExtLink=null, richHtmlUrl=null, mobilePdfUrl=null, reviewReport=null, pdfFirstPage=null, abstractGraph=null, abstractGraphContent=null, abstractVideo=null, citation=null, cebUrl=null, magXmlContent=null, mapNumber=null, authorCompany=null, fund=null, authors=null, authorsList=Jing-wen Gao, Yun-yu Qu, Zhi Zhang, Gang Shi, Yao Liu), CN=ArticleExt(id=1188049626180498105, articleId=1188049578868748895, tenantId=1146029695717560320, journalId=1185652524569653253, language=CN, title=包钢7
#高炉炉缸侧壁温度升高的分析与治理, columnId=1185882039552193444, journalTitle=包钢科技, columnName=生产实践与管理, runingTitle=null, highlight=null, articleAbstract=
文章分析了包钢7#高炉炉缸铁口区侧壁温度异常升高的原因,重点阐述了治理措施。高炉长期在高强度冶炼条件下,炉缸铁口区相对活跃,铁口深度控制不好,加剧了渣铁对铁口区炭砖的冲刷,铁口区炭砖受到侵蚀是导致7#高炉炉缸铁口区侧壁温度升高的根本原因。通过采取增加铁口区循环水量提高冷却强度、精心维护铁口、积极消除炉缸侧壁气隙、在装料制度上适当开放中心抑制边缘气流等措施,使7#高炉在没有降低冶炼强度、未减产的情况下,铁口区侧壁温度得到了有效控制。
, correspAuthors=null, authorNote=null, correspAuthorsNote=null, copyrightStatement=null, copyrightOwner=null, extLink=null, articleAbsUrl=null, sourceXml=uEqed8SzV2pOSWMEuLteqQ==, magXml=qGFovbdM0X5yG7OVWPkpDQ==, pdfUrl=null, pdf=4HENYTRsE7GEGmnWpgCbdg==, pdfFileSize=null, pdfExtLink=null, richHtmlUrl=null, mobilePdfUrl=null, reviewReport=null, pdfFirstPage=null, abstractGraph=null, abstractGraphContent=null, abstractVideo=null, citation=null, cebUrl=null, magXmlContent=XTnoGmE/1S6PuCj2IUBTKA==, mapNumber=null, authorCompany=null, fund=null, authors=
高靖文(1984-),男,内蒙古锡林郭勒盟人,高级工程师,现从事炼铁技术及管理工作。
, authorsList=高靖文, 曲玉云, 张智, 石钢, 刘耀)}, authors=[Author(id=1188503312732144554, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, orderNo=0, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1188503312811836331, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, authorId=1188503312732144554, language=EN, stringName=Jing-wen Gao, firstName=Jing-wen, middleName=null, lastName=Gao, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=null, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1188503312862167980, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, authorId=1188503312732144554, language=CN, stringName=高靖文, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=null, bio={"content":"
高靖文(1984-),男,内蒙古锡林郭勒盟人,高级工程师,现从事炼铁技术及管理工作。
"}, bioImg=null, bioContent=
高靖文(1984-),男,内蒙古锡林郭勒盟人,高级工程师,现从事炼铁技术及管理工作。
, aboutCorrespAuthor=null)}, companyList=null), Author(id=1188503312916693934, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, orderNo=1, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1188503312962831279, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, authorId=1188503312916693934, language=EN, stringName=Yun-yu Qu, firstName=Yun-yu, middleName=null, lastName=Qu, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=null, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1188503313067688880, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, authorId=1188503312916693934, language=CN, stringName=曲玉云, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=null, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=null), Author(id=1188503313118020530, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, orderNo=2, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1188503313185129395, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, authorId=1188503313118020530, language=EN, stringName=Zhi Zhang, firstName=Zhi, middleName=null, lastName=Zhang, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=null, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1188503313235461044, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, authorId=1188503313118020530, language=CN, stringName=张智, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=null, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=null), Author(id=1188503313294181302, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, orderNo=3, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1188503313340318647, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, authorId=1188503313294181302, language=EN, stringName=Gang Shi, firstName=Gang, middleName=null, lastName=Shi, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=null, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1188503313386455992, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, authorId=1188503313294181302, language=CN, stringName=石钢, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=null, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=null), Author(id=1188503313432593338, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, orderNo=4, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1188503313487119291, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, authorId=1188503313432593338, language=EN, stringName=Yao Liu, firstName=Yao, middleName=null, lastName=Liu, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=null, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1188503313554228156, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, authorId=1188503313432593338, language=CN, stringName=刘耀, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=null, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=null)], keywords=[Keyword(id=1188503313726194621, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, language=EN, orderNo=1, keyword=large blast furnace), Keyword(id=1188503313805886398, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, language=EN, orderNo=2, keyword=temperature of side wall at tap hole), Keyword(id=1188503313872995263, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, language=EN, orderNo=3, keyword=comprehensive treatment), Keyword(id=1188503313935909824, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, language=CN, orderNo=1, keyword=大型高炉), Keyword(id=1188503313994630081, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, language=CN, orderNo=2, keyword=铁口区侧壁温度), Keyword(id=1188503314057544642, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, language=CN, orderNo=3, keyword=综合治理)], refs=[Reference(id=1188503314665718729, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, doi=null, pmid=null, pmcid=null, year=2016, volume=39, issue=6, pageStart=48, pageEnd=50, url=null, language=null, rfNumber=[1], rfOrder=0, authorNames=李学斌, journalName=山西冶金, refType=null, unstructuredReference=李学斌. 邯宝2号高炉炉缸侧壁温度上升的治理实践[J].
山西冶金,
2016,
39(6):48-50., articleTitle=邯宝2号高炉炉缸侧壁温度上升的治理实践, refAbstract=null), Reference(id=1188503315642991562, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, doi=null, pmid=null, pmcid=null, year=2018, volume=37, issue=3, pageStart=40, pageEnd=42, url=null, language=null, rfNumber=[2], rfOrder=1, authorNames=文望龙, 穆红旺, 谭清涛, journalName=炼铁, refType=null, unstructuredReference=文望龙, 穆红旺, 谭清涛. 湘钢1号高炉炉缸侧壁温度升高的治理[J].
炼铁,
2018,
37(3):40-42., articleTitle=湘钢1号高炉炉缸侧壁温度升高的治理, refAbstract=null)], funds=null, companyList=[AuthorCompany(id=1188503312665035686, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, xref=null, ext=[AuthorCompanyExt(id=1188503312669229991, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, companyId=1188503312665035686, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=Iron-making Plant of Inner Mongolia Baotou Steel Rare Earth Steel Plate Co., Ltd., Baotou 014010, Inner Mongolia Autonomous Region, China), AuthorCompanyExt(id=1188503312677618600, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, companyId=1188503312665035686, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=内蒙古包钢稀土钢板材有限责任公司炼铁厂,内蒙古 包头 014010)])], figs=[ArticleFig(id=1188503314200150979, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, language=EN, label=null, caption=null, figureFileSmall=vcLAMhVYo32cm3CD7pZihg==, figureFileBig=wpIJhM2uhcXMNGPCbtCX3w==, tableContent=null), ArticleFig(id=1188503314254676932, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, language=CN, label=图1, caption=
焦炭反应后强度趋势图, figureFileSmall=vcLAMhVYo32cm3CD7pZihg==, figureFileBig=wpIJhM2uhcXMNGPCbtCX3w==, tableContent=null), ArticleFig(id=1188503314309202885, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, language=EN, label=null, caption=null, figureFileSmall=null, figureFileBig=null, tableContent=
| 时间 | 日产量 /(t·d-1) | 利用系数 /(t·m-3·d-1) | 燃料比 /(kg·t-1) | 富氧量 /(m3·h-1) | 焦炭负荷 /(t·t-1) | 休风率 /% |
| 2018年7月 | 8 346.0 | 2.016 | 591.94 | 14 072 | 3.70 | 0.22 |
| 2018年8月 | 8 832.5 | 2.136 | 572.23 | 16 406 | 3.80 | 0.37 |
| 2018年9月 | 8 830.5 | 2.131 | 570.38 | 15 304 | 3.86 | 0.16 |
| 2018年10月 | 6 645.5 | 1.647 | 592.63 | 14 642 | 3.63 | 2.75 |
| 2018年11月 | 8 840.3 | 2.132 | 555.05 | 16 950 | 3.80 | 0.07 |
| 2018年12月 | 8 100.1 | 2.140 | 571.75 | 15 149 | 3.88 | 8.78 |
| 7—12月平均 | 8 265.8 | 2.034 | 575.66 | 15 421 | 3.78 | 2.06 |
| 2019年1月 | 8 908.4 | 2.148 | 549.96 | 14 337 | 3.88 | 0.06 |
| 2019年2月 | 9 006.7 | 2.170 | 544.12 | 12 979 | 3.94 | 0 |
| 2019年3月 | 8 720.6 | 2.129 | 564.97 | 14 341 | 3.97 | 1.31 |
| 2019年4月 | 8 610.4 | 2.089 | 543.95 | 13 293 | 3.91 | 0.69 |
| 2019年5月 | 9 041.0 | 2.179 | 536.42 | 15 866 | 4.07 | 0 |
| 2019年6月 | 9 166.9 | 2.212 | 535.22 | 14 921 | 4.14 | 0.15 |
| 1—6月平均 | 8 909.0 | 2.155 | 545.77 | 14 290 | 3.99 | 0.37 |
2019年1—6月较 2018年6—12月 | 643.2 | 0.121 | -29.89 | -1 131 | 0.21 | -1.69 |
), ArticleFig(id=1188503314393088966, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, language=CN, label=表1, caption=
包钢7#高炉主要技术经济指标
, figureFileSmall=null, figureFileBig=null, tableContent=
| 时间 | 日产量 /(t·d-1) | 利用系数 /(t·m-3·d-1) | 燃料比 /(kg·t-1) | 富氧量 /(m3·h-1) | 焦炭负荷 /(t·t-1) | 休风率 /% |
| 2018年7月 | 8 346.0 | 2.016 | 591.94 | 14 072 | 3.70 | 0.22 |
| 2018年8月 | 8 832.5 | 2.136 | 572.23 | 16 406 | 3.80 | 0.37 |
| 2018年9月 | 8 830.5 | 2.131 | 570.38 | 15 304 | 3.86 | 0.16 |
| 2018年10月 | 6 645.5 | 1.647 | 592.63 | 14 642 | 3.63 | 2.75 |
| 2018年11月 | 8 840.3 | 2.132 | 555.05 | 16 950 | 3.80 | 0.07 |
| 2018年12月 | 8 100.1 | 2.140 | 571.75 | 15 149 | 3.88 | 8.78 |
| 7—12月平均 | 8 265.8 | 2.034 | 575.66 | 15 421 | 3.78 | 2.06 |
| 2019年1月 | 8 908.4 | 2.148 | 549.96 | 14 337 | 3.88 | 0.06 |
| 2019年2月 | 9 006.7 | 2.170 | 544.12 | 12 979 | 3.94 | 0 |
| 2019年3月 | 8 720.6 | 2.129 | 564.97 | 14 341 | 3.97 | 1.31 |
| 2019年4月 | 8 610.4 | 2.089 | 543.95 | 13 293 | 3.91 | 0.69 |
| 2019年5月 | 9 041.0 | 2.179 | 536.42 | 15 866 | 4.07 | 0 |
| 2019年6月 | 9 166.9 | 2.212 | 535.22 | 14 921 | 4.14 | 0.15 |
| 1—6月平均 | 8 909.0 | 2.155 | 545.77 | 14 290 | 3.99 | 0.37 |
2019年1—6月较 2018年6—12月 | 643.2 | 0.121 | -29.89 | -1 131 | 0.21 | -1.69 |
), ArticleFig(id=1188503314456003527, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, language=EN, label=null, caption=null, figureFileSmall=null, figureFileBig=null, tableContent=
| 日期 | 钻口深度/m | 打泥量/L | 炮泥类型 |
| 1月15日 | 2.10 | 25 | 含Ti炮泥 |
| 1月16日 | 2.30 | 180 | 含Ti炮泥 |
| 1月17日 | 2.90 | 220 | 含Ti炮泥 |
| 1月18日 | 2.60 | 220 | 含Ti炮泥 |
| 1月21日 | 2.45 | 220 | 含Ti炮泥 |
| 1月23日 | 2.55 | 180 | 瑞尔炮泥 |
| 1月25日 | 2.60 | 220 | 瑞尔炮泥 |
| 1月30日 | 2.40 | 220 | 瑞尔炮泥 |
| 1月31日 | 2.20 | 44 | 瑞尔炮泥 |
| 2月1日 | 2.50 | 221 | 瑞尔炮泥 |
| 2月3日 | 2.90 | 223 | 瑞尔炮泥 |
| 2月6日 | 2.80 | 220 | 瑞尔炮泥 |
| 2月8日 | 2.80 | 220 | 瑞尔炮泥 |
| 2月13日 | 2.60 | 221 | 瑞尔炮泥 |
| 2月15日 | 2.50 | 180 | 普通炮泥 |
| 2月18日 | 2.40 | 224 | 普通炮泥 |
| 2月20日 | 2.50 | 200 | 普通炮泥 |
), ArticleFig(id=1188503314523112392, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049578868748895, language=CN, label=表2, caption=
钻口深度及打泥量
, figureFileSmall=null, figureFileBig=null, tableContent=
| 日期 | 钻口深度/m | 打泥量/L | 炮泥类型 |
| 1月15日 | 2.10 | 25 | 含Ti炮泥 |
| 1月16日 | 2.30 | 180 | 含Ti炮泥 |
| 1月17日 | 2.90 | 220 | 含Ti炮泥 |
| 1月18日 | 2.60 | 220 | 含Ti炮泥 |
| 1月21日 | 2.45 | 220 | 含Ti炮泥 |
| 1月23日 | 2.55 | 180 | 瑞尔炮泥 |
| 1月25日 | 2.60 | 220 | 瑞尔炮泥 |
| 1月30日 | 2.40 | 220 | 瑞尔炮泥 |
| 1月31日 | 2.20 | 44 | 瑞尔炮泥 |
| 2月1日 | 2.50 | 221 | 瑞尔炮泥 |
| 2月3日 | 2.90 | 223 | 瑞尔炮泥 |
| 2月6日 | 2.80 | 220 | 瑞尔炮泥 |
| 2月8日 | 2.80 | 220 | 瑞尔炮泥 |
| 2月13日 | 2.60 | 221 | 瑞尔炮泥 |
| 2月15日 | 2.50 | 180 | 普通炮泥 |
| 2月18日 | 2.40 | 224 | 普通炮泥 |
| 2月20日 | 2.50 | 200 | 普通炮泥 |
)], attaches=null, journal=Journal(id=1185652280146587652, delFlag=0, nameCn=包钢科技, nameEn=Science & Technology of Baotou Steel, nameHistory1=null, nameHistory2=null, issn=1009-5438, eissn=null, cn=15-1210/TF, coden=null, periodic=1, language=CN, oaType=null, ccby=null, superviseOffice=null, ownerOffice=null, pubOffice=null, editorOffice=null, officeType=null, aims=null, clcCode=null, officeProv=null, officeCity=null, officeAddr=null, officeZip=null, officeEmail=null, officePhone=null, editDirector=null, officeDirector=null, officeDirectorPhone=null, officeStaffNum=null, officeEmpNum=null, coverPicUrl=MuxxMe9Pr9qgO8IAocuQTg==, journalPrice=null, startedYear=null, abbrevIsoEn=null, journalRemark=null, publicationField=null, createdTime=1760611131943, updatedTime=1761728493461, createdBy=18614031015, updatedBy=13701087609, firstLetterCn=B, firstLetterEn=B, subjectCode=Engineering, subjectName=Engineering, subjectCodeEn=Engineering, subjectNameEn=null, picCn=MuxxMe9Pr9qgO8IAocuQTg==, picEn=ou3AszwYb0n2VtOVtaZ2lw==, jcr=null, cjcr=null, exts=[JournalExt(id=1190338834354245756, language=CN, name=包钢科技, nameHistory1=null, nameHistory2=null, managedBy=, sponsoredBy=, publishedBy=, editorOffice=, officeProv=null, officeCity=null, officeAddr=, officeZip=, editDirector=, officeDirector=null, officePhone=null, coverPicUrl=null, journalRemark=, submitArticleUrl=null, websiteUrl=, createdTime=1761728493536, updatedTime=1761728493536, createdBy=13701087609, updatedBy=13701087609, submissionGuidelinesUrl=, submissionAuthorUrl=https://bgkj.chinajournal.net.cn/EditorDN/index.aspx?t=1, submissionEditorUrl=https://bgkj.chinajournal.net.cn/EditorDN/index.aspx?t=3, submissionReviewUrl=https://bgkj.chinajournal.net.cn/EditorDN/index.aspx?t=2, submissionCeEditorUrl=, submissionAeEditorUrl=, option={"copyright":""}), JournalExt(id=1190338834408771709, language=EN, name=Science & Technology of Baotou Steel, nameHistory1=null, nameHistory2=null, managedBy=, sponsoredBy=, publishedBy=, editorOffice=, officeProv=null, officeCity=null, officeAddr=, officeZip=, editDirector=, officeDirector=null, officePhone=null, coverPicUrl=null, journalRemark=, submitArticleUrl=null, websiteUrl=, createdTime=1761728493549, updatedTime=1761728493549, createdBy=13701087609, updatedBy=13701087609, submissionGuidelinesUrl=, submissionAuthorUrl=https://bgkj.chinajournal.net.cn/EditorDN/index.aspx?t=1, submissionEditorUrl=https://bgkj.chinajournal.net.cn/EditorDN/index.aspx?t=3, submissionReviewUrl=https://bgkj.chinajournal.net.cn/EditorDN/index.aspx?t=2, submissionCeEditorUrl=, submissionAeEditorUrl=, option={"copyright":""})], databaseList=null, tenantJournalId=1185652524569653253, websiteList=[Website(id=1185655046684423052, webName=null, webTitle=null, webDomain=null, webCopyrigh=null, webIpcNo=null, seoTitle=null, seoKeywords=null, seoDescription=null, tenantJournalId=null, journalId=1185652524569653253, journalNameCn=null, journalNameEn=null, grayFlag=null, tenantId=1146029695717560320, platformId=null, journalGroupId=null, journalGroupNameCn=null, journalGroupNameEn=null, type=1, domain=https://castjournals.cast.org.cn/joweb/bgkj/CN, language=CN, createTime=1760611791535, createBy=18614031015, updateTime=1760611862376, updateBy=18614031015, name=包钢科技, tplId=1146099689490845704, title=包钢科技, delFlag=0, indexPage=/home, props=[WebsiteProps(id=1185675258741801724, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046684423052, code=articleTextType, value=kx, createTime=1760616610465, updateTime=1760616610465, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675258708247289, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046684423052, code=banner, value=null, createTime=1760616610457, updateTime=1760616610457, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675258699858680, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046684423052, code=logo, value=https://castjournals.cast.org.cn/joweb/bgkj/CN/file/pic?fileId=nthji6+GG9SlnD/dssvyKA==, createTime=1760616610455, updateTime=1760616610455, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675258737607419, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046684423052, code=picServerUrl, value=https://castjournals.cast.org.cn/joweb/bgkj/CN/file/pic, createTime=1760616610464, updateTime=1760616610464, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675258729218810, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046684423052, code=staticResourcePath, value=https://castjournals.cast.org.cn/joweb/cast_kjdb_cn_619/, createTime=1760616610462, updateTime=1760616610462, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675258750190333, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046684423052, code=themeColor, value=null, createTime=1760616610467, updateTime=1760616610467, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675258758578942, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046684423052, code=themeStyle, value=null, createTime=1760616610469, updateTime=1760616610469, creator=18614031015, updator=18614031015)]), Website(id=1185655046801863567, webName=null, webTitle=null, webDomain=null, webCopyrigh=null, webIpcNo=null, seoTitle=null, seoKeywords=null, seoDescription=null, tenantJournalId=null, journalId=1185652524569653253, journalNameCn=null, journalNameEn=null, grayFlag=null, tenantId=1146029695717560320, platformId=null, journalGroupId=null, journalGroupNameCn=null, journalGroupNameEn=null, type=1, domain=https://castjournals.cast.org.cn/joweb/bgkj/EN, language=EN, createTime=1760611791563, createBy=18614031015, updateTime=1760611898113, updateBy=18614031015, name=包钢科技-英文, tplId=1146101810881728533, title=Science & Technology of Baotou Steel, delFlag=0, indexPage=/home, props=[WebsiteProps(id=1185675300932305667, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046801863567, code=articleTextType, value=kx, createTime=1760616620524, updateTime=1760616620524, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675300907139840, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046801863567, code=banner, value=null, createTime=1760616620518, updateTime=1760616620518, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675300898751231, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046801863567, code=logo, value=https://castjournals.cast.org.cn/joweb/bgkj/EN/file/pic?fileId=nthji6+GG9SlnD/dssvyKA==, createTime=1760616620516, updateTime=1760616620516, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675300923917058, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046801863567, code=picServerUrl, value=https://castjournals.cast.org.cn/joweb/bgkj/EN/file/pic, createTime=1760616620522, updateTime=1760616620522, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675300915528449, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046801863567, code=staticResourcePath, value=https://castjournals.cast.org.cn/joweb/cast_kjdb_en_623/, createTime=1760616620520, updateTime=1760616620520, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675300936499972, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046801863567, code=themeColor, value=null, createTime=1760616620525, updateTime=1760616620525, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675300999414533, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046801863567, code=themeStyle, value=null, createTime=1760616620540, updateTime=1760616620540, creator=18614031015, updator=18614031015)])], journalTitle=包钢科技, weixinUrl=null, journalUrl=null, iacademicId=null, status=1, seqNo=null, journalTitleEn=Science & Technology of Baotou Steel, journalPhotoCn=MuxxMe9Pr9qgO8IAocuQTg==, journalPhotoEn=ou3AszwYb0n2VtOVtaZ2lw==, journalFirstLetter=B, journalRecommend=null, journalNew=null, journalCollection=1, jcrJf=null, cjcrJf=null, jcrJfStr=null, cjcrJfStr=null, submissionFirstDecision=null, sciSubjectClassification=null, casSubjectClassification=null, citeScore=null, totalCitationFrequency=null, icpCode=null, psCode=null, advertisingLicenseCode=null, copyrightInformation=null, country=null, option=, provinceCode=null, provinceName=null, collectFlag=false), detailUrlCn=https://castjournals.cast.org.cn/joweb/bgkj/CN/Y2024/V50/I1/20, detailUrlEn=https://castjournals.cast.org.cn/joweb/bgkj/EN/Y2024/V50/I1/20, pdfUrlCn=https://castjournals.cast.org.cn/joweb/bgkj/CN/PDF/Y2024/V50/I1/20, pdfUrlEn=https://castjournals.cast.org.cn/joweb/bgkj/EN/PDF/Y2024/V50/I1/20, aliStartDate=null, aliEndDate=null, collectionFlag=false, citedCount=null, citedUrl=null, reference=null)