Article(id=1188049105763840093, tenantId=1146029695717560320, journalId=1185652524569653253, issueId=1188049099627574244, articleNumber=1009-5438(2024)02-0032-04, orderNo=null, doi=null, pmid=null, cstr=null, oa=null, hot=null, price=null, onlineType=0, articleFormat=0, articleType=null, articleTypeStr=null, receivedDate=1706371200000, receivedDateStr=2024-01-28, revisedDate=null, revisedDateStr=null, acceptedDate=null, acceptedDateStr=null, onlineDate=1761182579698, onlineDateStr=2025-10-23, pubDate=1713974400000, pubDateStr=2024-04-25, doiRegisterDate=null, doiRegisterDateStr=null, onlineIssueDate=1761182579698, onlineIssueDateStr=2025-10-23, onlineJustAcceptDate=null, onlineJustAcceptDateStr=null, onlineFirstDate=null, onlineFirstDateStr=null, sourceXml=null, magXml=null, createTime=1761182579698, creator=13701087609, updateTime=1761182579698, updator=13701087609, issue=Issue{id=1188049099627574244, tenantId=1146029695717560320, journalId=1185652524569653253, year='2024', volume='50', issue='2', pageStart='1', pageEnd='98', issueExtLink='null', onlineDate='null', pubDate='null', beforeIssueId=null, nextIssueId=null, price=null, status=1, issueComplete=1, articleOrder=1, issueType=-1, specialIssue=null, createTime=1761182578236, creator=13701087609, updateTime=1761291001661, updator=13701087609, preIssue=null, nextIssue=null, ext={EN=IssueExt(id=1188503860504052243, tenantId=1146029695717560320, journalId=1185652524569653253, issueId=1188049099627574244, language=EN, specialIssueTitle=, coverIllustrator=null, specialIssueEditor=, specialIssueAbout=), CN=IssueExt(id=1188503860504052244, tenantId=1146029695717560320, journalId=1185652524569653253, issueId=1188049099627574244, language=CN, specialIssueTitle=, coverIllustrator=null, specialIssueEditor=, specialIssueAbout=)}, issueFiles=null}, startPage=32, endPage=35, ext={EN=ArticleExt(id=1188049106061635681, articleId=1188049105763840093, tenantId=1146029695717560320, journalId=1185652524569653253, language=EN, title=Analysis and Improvement on Cracking of Cold Rolled Sheet SPCC, columnId=1187095652984042303, journalTitle=Science & Technology of Baotou Steel, columnName=Variety Quality and Experimental Study, runingTitle=null, highlight=null, articleAbstract=

The feedback of user is that the elongation of cold rolled sheet with cold rolled base material SPCC manufactured by 2 250 mm production line after cold rolling and annealing is low, part of flow forming is not easily to form in punch forming process and cracking rate is higher. The cause analysis showed that its high Mn content was one of the causes for slightly higher strength of steel strip so that elongation was low and steel strip was easy to crack; cooling modes of the two production lines were different, the cooling mode of preconcentration was adopted by 2 250 mm production line and the cooling mode of predispersion was adopted by CSP production line so that the strength of hot rolled steel strip manufactured by 2 250 mm production line was slightly higher, elongation was low and steel strip was easy to crack. The elongation of hot rolled steel strip manufactured with raw materials with thickness of 3.0~5.0 mm by 2 250 mm production line is lower than that of hot rolled steel strip manufactured by CSP production line so that the elongation of cold rolled steel strip after cold rolling and annealing is also slightly higher due to the “heredity” of rolling.

, correspAuthors=null, authorNote=null, correspAuthorsNote=null, copyrightStatement=null, copyrightOwner=null, extLink=null, articleAbsUrl=null, sourceXml=null, magXml=null, pdfUrl=null, pdf=null, pdfFileSize=null, pdfExtLink=null, richHtmlUrl=null, mobilePdfUrl=null, reviewReport=null, pdfFirstPage=null, abstractGraph=null, abstractGraphContent=null, abstractVideo=null, citation=null, cebUrl=null, magXmlContent=null, mapNumber=null, authorCompany=null, fund=null, authors=null, authorsList=Dong-qing Guo, Shao-bing Wang, Li Huang, Xiong Yang), CN=ArticleExt(id=1188049178744729798, articleId=1188049105763840093, tenantId=1146029695717560320, journalId=1185652524569653253, language=CN, title=冷轧板SPCC开裂分析及改进, columnId=1185887584472417142, journalTitle=包钢科技, columnName=品种质量与试验研究, runingTitle=null, highlight=null, articleAbstract=

2 250 mm生产线生产的冷轧基料SPCC冷轧退火后的冷轧板,用户反映其成品延伸率低,在冲压成型过程中旋压部位不易成型,开裂率较高。针对此种情况进行原因分析,2 250 mm生产线生产的冷轧钢带SPCC Mn元素含量高是造成钢带强度略高的原因之一,钢带强度高,延伸率低,钢带易开裂;两条生产线冷却模式不同,2 250 mm生产线采用前集中冷却模式,CSP生产线采用前分散冷却模式,采用前集中冷却模式会造成热轧钢带强度略高,延伸率低,钢带易开裂。对应3.0~5.0 mm厚原料2 250 mm生产线生产的热轧钢带延伸率低于CSP生产线生产的热轧钢带,由于轧制的“遗传性”,热轧钢带延伸率高一般经冷轧退火后冷轧钢带延伸率也略高。

, correspAuthors=null, authorNote=null, correspAuthorsNote=null, copyrightStatement=null, copyrightOwner=null, extLink=null, articleAbsUrl=null, sourceXml=BCZKHgeuWt18LS8AYITe6A==, magXml=clbs0Njv+o3gsWWF3spCEg==, pdfUrl=null, pdf=iXzJT7QKU5uMx1fCREc0kQ==, pdfFileSize=null, pdfExtLink=null, richHtmlUrl=null, mobilePdfUrl=null, reviewReport=null, pdfFirstPage=null, abstractGraph=null, abstractGraphContent=null, abstractVideo=null, citation=null, cebUrl=null, magXmlContent=UBYoSGtHn3I9x5W8cwUk7w==, mapNumber=null, authorCompany=null, fund=null, authors=

郭冬青(1988-),女,内蒙古乌兰察布市人,硕士,高级工程师,现从事板材新产品研发工作。

, authorsList=郭冬青, 王少炳, 黄利, 杨雄)}, authors=[Author(id=1188503098415789035, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, orderNo=0, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1188503098478703599, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, authorId=1188503098415789035, language=EN, stringName=Dong-qing Guo, firstName=Dong-qing, middleName=null, lastName=Guo, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=null, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1188503098638087153, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, authorId=1188503098415789035, language=CN, stringName=郭冬青, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=null, bio={"content":"

郭冬青(1988-),女,内蒙古乌兰察布市人,硕士,高级工程师,现从事板材新产品研发工作。

"}, bioImg=null, bioContent=

郭冬青(1988-),女,内蒙古乌兰察布市人,硕士,高级工程师,现从事板材新产品研发工作。

, aboutCorrespAuthor=null)}, companyList=null), Author(id=1188503098709390325, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, orderNo=1, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1188503098843608057, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, authorId=1188503098709390325, language=EN, stringName=Shao-bing Wang, firstName=Shao-bing, middleName=null, lastName=Wang, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=null, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1188503098910716922, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, authorId=1188503098709390325, language=CN, stringName=王少炳, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=null, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=null), Author(id=1188503099028157438, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, orderNo=2, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1188503099099460606, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, authorId=1188503099028157438, language=EN, stringName=Li Huang, firstName=Li, middleName=null, lastName=Huang, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=null, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1188503099204317184, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, authorId=1188503099028157438, language=CN, stringName=黄利, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=null, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=null), Author(id=1188503099296591874, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, orderNo=3, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1188503099372089348, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, authorId=1188503099296591874, language=EN, stringName=Xiong Yang, firstName=Xiong, middleName=null, lastName=Yang, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=null, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1188503099443392518, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, authorId=1188503099296591874, language=CN, stringName=杨雄, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=null, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=null)], keywords=[Keyword(id=1188503099598581769, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, language=EN, orderNo=1, keyword=CSP production line), Keyword(id=1188503099678273547, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, language=EN, orderNo=2, keyword=2 250 mm production line), Keyword(id=1188503099762159629, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, language=EN, orderNo=3, keyword=property), Keyword(id=1188503099833462798, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, language=EN, orderNo=4, keyword=technology), Keyword(id=1188503099980263440, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, language=CN, orderNo=1, keyword=CSP生产线), Keyword(id=1188503100106092562, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, language=CN, orderNo=2, keyword=2 250 mm生产线), Keyword(id=1188503100206755860, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, language=CN, orderNo=3, keyword=性能), Keyword(id=1188503100307419158, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, language=CN, orderNo=4, keyword=工艺)], refs=[Reference(id=1188503101251137571, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, doi=null, pmid=null, pmcid=null, year=2011, volume=34, issue=S1, pageStart=158, pageEnd=160, url=null, language=null, rfNumber=[1], rfOrder=0, authorNames=汪凤, 范玉然, 尹长华, journalName=金属热处理, refType=null, unstructuredReference=汪凤, 范玉然, 尹长华, 等. Q235B钢板冷弯开裂原因分析[J]. 金属热处理, 2011, 34(S1):158-160., articleTitle=Q235B钢板冷弯开裂原因分析, refAbstract=null), Reference(id=1188503101330829348, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, doi=null, pmid=null, pmcid=null, year=2007, volume=null, issue=null, pageStart=null, pageEnd=null, url=null, language=null, rfNumber=[2], rfOrder=1, authorNames=张中平, journalName=高强汽车大梁钢微观组织控制与TMCP工艺开发, refType=null, unstructuredReference=张中平. 高强汽车大梁钢微观组织控制与TMCP工艺开发[D]. 沈阳: 东北大学, 2007., articleTitle=null, refAbstract=null), Reference(id=1188503102366822437, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, doi=null, pmid=null, pmcid=null, year=2015, volume=43, issue=1, pageStart=21, pageEnd=23, url=null, language=null, rfNumber=[3], rfOrder=2, authorNames=刘跃飞, journalName=金属材料与冶金工程, refType=null, unstructuredReference=刘跃飞. Q345B热轧钢板加工开裂的原因分析[J]. 金属材料与冶金工程, 2015, 43(1):21-23., articleTitle=Q345B热轧钢板加工开裂的原因分析, refAbstract=null), Reference(id=1188503102438125606, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, doi=null, pmid=null, pmcid=null, year=1996, volume=null, issue=4, pageStart=1, pageEnd=9, url=null, language=null, rfNumber=[4], rfOrder=3, authorNames=许洪新, journalName=太钢科技, refType=null, unstructuredReference=许洪新. 汽车用钢研究开发的现状和发展[J]. 太钢科技, 1996(4):1-9., articleTitle=汽车用钢研究开发的现状和发展, refAbstract=null), Reference(id=1188503102501040167, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, doi=null, pmid=null, pmcid=null, year=1991, volume=null, issue=3, pageStart=13, pageEnd=16, url=null, language=null, rfNumber=[5], rfOrder=4, authorNames=李明久, journalName=鞍钢技术, refType=null, unstructuredReference=李明久. 08Al冷板性能升级的开发研究[J]. 鞍钢技术, 1991(3):13-16., articleTitle=08Al冷板性能升级的开发研究, refAbstract=null), Reference(id=1188503102639452200, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, doi=null, pmid=null, pmcid=null, year=1991, volume=null, issue=3, pageStart=13, pageEnd=16, url=null, language=null, rfNumber=[6], rfOrder=5, authorNames=常军, 张开华, 程兴德, journalName=钢铁钒钛, refType=null, unstructuredReference=常军, 张开华, 程兴德, 等. 终轧温度和卷取温度对低碳铝镇静钢性能的影响[J]. 钢铁钒钛, 1991(3):13-16., articleTitle=终轧温度和卷取温度对低碳铝镇静钢性能的影响, refAbstract=null)], funds=null, companyList=[AuthorCompany(id=1188503098340291558, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, xref=null, ext=[AuthorCompanyExt(id=1188503098348680167, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, companyId=1188503098340291558, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=Technical Center of Inner Mongolia Baotou Steel Union Co., Ltd., Baotou 014010, Inner Mongolia Autonomous Region, China), AuthorCompanyExt(id=1188503098357068776, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, companyId=1188503098340291558, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=内蒙古包钢钢联股份有限公司技术中心,内蒙古 包头 014010)])], figs=[ArticleFig(id=1188503100454219801, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, language=EN, label=null, caption=null, figureFileSmall=xbVSCaUZ5YdqIFsP6fL4xw==, figureFileBig=lVLkK/IwDcvTIyAoMHtzjg==, tableContent=null), ArticleFig(id=1188503100521328666, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, language=CN, label=图1, caption=冷轧板力学性能对比图, figureFileSmall=xbVSCaUZ5YdqIFsP6fL4xw==, figureFileBig=lVLkK/IwDcvTIyAoMHtzjg==, tableContent=null), ArticleFig(id=1188503100580048924, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, language=EN, label=null, caption=null, figureFileSmall=auAMxVeWF+sBgX7gEvd3Mg==, figureFileBig=NucnGoWUknUd+ifZY4I3LQ==, tableContent=null), ArticleFig(id=1188503100642963486, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, language=CN, label=图2, caption=冷轧基料力学性能对比图, figureFileSmall=auAMxVeWF+sBgX7gEvd3Mg==, figureFileBig=NucnGoWUknUd+ifZY4I3LQ==, tableContent=null), ArticleFig(id=1188503100710072351, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, language=EN, label=null, caption=null, figureFileSmall=null, figureFileBig=null, tableContent=
料源 C Si Mn P S Alt
2 250 mm生产线 0.03~0.06 ≤0.03 0.15~0.25 ≤0.015 ≤0.015 0.020~0.033
CSP生产线 0.03~0.05 ≤0.03 0.10~0.20 ≤0.020 ≤0.009 0.025~0.035
), ArticleFig(id=1188503100798152736, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, language=CN, label=表1, caption=

化学成分平均值(质量分数) %

, figureFileSmall=null, figureFileBig=null, tableContent=
料源 C Si Mn P S Alt
2 250 mm生产线 0.03~0.06 ≤0.03 0.15~0.25 ≤0.015 ≤0.015 0.020~0.033
CSP生产线 0.03~0.05 ≤0.03 0.10~0.20 ≤0.020 ≤0.009 0.025~0.035
), ArticleFig(id=1188503100865261601, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, language=EN, label=null, caption=null, figureFileSmall=null, figureFileBig=null, tableContent=
2 250 mm生产线 CSP生产线
厚度/mm 终轧温度/℃ 卷取温度/℃ 冷却模式 厚度/mm 终轧温度/℃ 卷取温度/℃ 冷却模式
>1.2~3.0 900±15 600±15 前、集中 >2.0~2.5 900±10 590±10 前、分散
>2.5~3.0 900±10 580±10 前、分散
>3.0~6.0 890±15 580±15 前、集中 >3.0~4.0 900±10 570±10 前、分散
>4.0~6.0 900±10 570±10 前、分散
), ArticleFig(id=1188503100961730594, tenantId=1146029695717560320, journalId=1185652524569653253, articleId=1188049105763840093, language=CN, label=表2, caption=

实际工艺参数对比

, figureFileSmall=null, figureFileBig=null, tableContent=
2 250 mm生产线 CSP生产线
厚度/mm 终轧温度/℃ 卷取温度/℃ 冷却模式 厚度/mm 终轧温度/℃ 卷取温度/℃ 冷却模式
>1.2~3.0 900±15 600±15 前、集中 >2.0~2.5 900±10 590±10 前、分散
>2.5~3.0 900±10 580±10 前、分散
>3.0~6.0 890±15 580±15 前、集中 >3.0~4.0 900±10 570±10 前、分散
>4.0~6.0 900±10 570±10 前、分散
)], attaches=null, journal=Journal(id=1185652280146587652, delFlag=0, nameCn=包钢科技, nameEn=Science & Technology of Baotou Steel, nameHistory1=null, nameHistory2=null, issn=1009-5438, eissn=null, cn=15-1210/TF, coden=null, periodic=1, language=CN, oaType=null, ccby=null, superviseOffice=null, ownerOffice=null, pubOffice=null, editorOffice=null, officeType=null, aims=null, clcCode=null, officeProv=null, officeCity=null, officeAddr=null, officeZip=null, officeEmail=null, officePhone=null, editDirector=null, officeDirector=null, officeDirectorPhone=null, officeStaffNum=null, officeEmpNum=null, coverPicUrl=MuxxMe9Pr9qgO8IAocuQTg==, journalPrice=null, startedYear=null, abbrevIsoEn=null, journalRemark=null, publicationField=null, createdTime=1760611131943, updatedTime=1761728493461, createdBy=18614031015, updatedBy=13701087609, firstLetterCn=B, firstLetterEn=B, subjectCode=Engineering, subjectName=Engineering, subjectCodeEn=Engineering, subjectNameEn=null, picCn=MuxxMe9Pr9qgO8IAocuQTg==, picEn=ou3AszwYb0n2VtOVtaZ2lw==, jcr=null, cjcr=null, exts=[JournalExt(id=1190338834354245756, language=CN, name=包钢科技, nameHistory1=null, nameHistory2=null, managedBy=, sponsoredBy=, publishedBy=, editorOffice=, officeProv=null, officeCity=null, officeAddr=, officeZip=, editDirector=, officeDirector=null, officePhone=null, coverPicUrl=null, journalRemark=, submitArticleUrl=null, websiteUrl=, createdTime=1761728493536, updatedTime=1761728493536, createdBy=13701087609, updatedBy=13701087609, submissionGuidelinesUrl=, submissionAuthorUrl=https://bgkj.chinajournal.net.cn/EditorDN/index.aspx?t=1, submissionEditorUrl=https://bgkj.chinajournal.net.cn/EditorDN/index.aspx?t=3, submissionReviewUrl=https://bgkj.chinajournal.net.cn/EditorDN/index.aspx?t=2, submissionCeEditorUrl=, submissionAeEditorUrl=, option={"copyright":""}), JournalExt(id=1190338834408771709, language=EN, name=Science & Technology of Baotou Steel, nameHistory1=null, nameHistory2=null, managedBy=, sponsoredBy=, publishedBy=, editorOffice=, officeProv=null, officeCity=null, officeAddr=, officeZip=, editDirector=, officeDirector=null, officePhone=null, coverPicUrl=null, journalRemark=, submitArticleUrl=null, websiteUrl=, createdTime=1761728493549, updatedTime=1761728493549, createdBy=13701087609, updatedBy=13701087609, submissionGuidelinesUrl=, submissionAuthorUrl=https://bgkj.chinajournal.net.cn/EditorDN/index.aspx?t=1, submissionEditorUrl=https://bgkj.chinajournal.net.cn/EditorDN/index.aspx?t=3, submissionReviewUrl=https://bgkj.chinajournal.net.cn/EditorDN/index.aspx?t=2, submissionCeEditorUrl=, submissionAeEditorUrl=, option={"copyright":""})], databaseList=null, tenantJournalId=1185652524569653253, websiteList=[Website(id=1185655046684423052, webName=null, webTitle=null, webDomain=null, webCopyrigh=null, webIpcNo=null, seoTitle=null, seoKeywords=null, seoDescription=null, tenantJournalId=null, journalId=1185652524569653253, journalNameCn=null, journalNameEn=null, grayFlag=null, tenantId=1146029695717560320, platformId=null, journalGroupId=null, journalGroupNameCn=null, journalGroupNameEn=null, type=1, domain=https://castjournals.cast.org.cn/joweb/bgkj/CN, language=CN, createTime=1760611791535, createBy=18614031015, updateTime=1760611862376, updateBy=18614031015, name=包钢科技, tplId=1146099689490845704, title=包钢科技, delFlag=0, indexPage=/home, props=[WebsiteProps(id=1185675258741801724, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046684423052, code=articleTextType, value=kx, createTime=1760616610465, updateTime=1760616610465, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675258708247289, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046684423052, code=banner, value=null, createTime=1760616610457, updateTime=1760616610457, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675258699858680, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046684423052, code=logo, value=https://castjournals.cast.org.cn/joweb/bgkj/CN/file/pic?fileId=nthji6+GG9SlnD/dssvyKA==, createTime=1760616610455, updateTime=1760616610455, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675258737607419, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046684423052, code=picServerUrl, value=https://castjournals.cast.org.cn/joweb/bgkj/CN/file/pic, createTime=1760616610464, updateTime=1760616610464, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675258729218810, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046684423052, code=staticResourcePath, value=https://castjournals.cast.org.cn/joweb/cast_kjdb_cn_619/, createTime=1760616610462, updateTime=1760616610462, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675258750190333, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046684423052, code=themeColor, value=null, createTime=1760616610467, updateTime=1760616610467, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675258758578942, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046684423052, code=themeStyle, value=null, createTime=1760616610469, updateTime=1760616610469, creator=18614031015, updator=18614031015)]), Website(id=1185655046801863567, webName=null, webTitle=null, webDomain=null, webCopyrigh=null, webIpcNo=null, seoTitle=null, seoKeywords=null, seoDescription=null, tenantJournalId=null, journalId=1185652524569653253, journalNameCn=null, journalNameEn=null, grayFlag=null, tenantId=1146029695717560320, platformId=null, journalGroupId=null, journalGroupNameCn=null, journalGroupNameEn=null, type=1, domain=https://castjournals.cast.org.cn/joweb/bgkj/EN, language=EN, createTime=1760611791563, createBy=18614031015, updateTime=1760611898113, updateBy=18614031015, name=包钢科技-英文, tplId=1146101810881728533, title=Science & Technology of Baotou Steel, delFlag=0, indexPage=/home, props=[WebsiteProps(id=1185675300932305667, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046801863567, code=articleTextType, value=kx, createTime=1760616620524, updateTime=1760616620524, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675300907139840, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046801863567, code=banner, value=null, createTime=1760616620518, updateTime=1760616620518, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675300898751231, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046801863567, code=logo, value=https://castjournals.cast.org.cn/joweb/bgkj/EN/file/pic?fileId=nthji6+GG9SlnD/dssvyKA==, createTime=1760616620516, updateTime=1760616620516, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675300923917058, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046801863567, code=picServerUrl, value=https://castjournals.cast.org.cn/joweb/bgkj/EN/file/pic, createTime=1760616620522, updateTime=1760616620522, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675300915528449, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046801863567, code=staticResourcePath, value=https://castjournals.cast.org.cn/joweb/cast_kjdb_en_623/, createTime=1760616620520, updateTime=1760616620520, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675300936499972, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046801863567, code=themeColor, value=null, createTime=1760616620525, updateTime=1760616620525, creator=18614031015, updator=18614031015), WebsiteProps(id=1185675300999414533, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1185655046801863567, code=themeStyle, value=null, createTime=1760616620540, updateTime=1760616620540, creator=18614031015, updator=18614031015)])], journalTitle=包钢科技, weixinUrl=null, journalUrl=null, iacademicId=null, status=1, seqNo=null, journalTitleEn=Science & Technology of Baotou Steel, journalPhotoCn=MuxxMe9Pr9qgO8IAocuQTg==, journalPhotoEn=ou3AszwYb0n2VtOVtaZ2lw==, journalFirstLetter=B, journalRecommend=null, journalNew=null, journalCollection=1, jcrJf=null, cjcrJf=null, jcrJfStr=null, cjcrJfStr=null, submissionFirstDecision=null, sciSubjectClassification=null, casSubjectClassification=null, citeScore=null, totalCitationFrequency=null, icpCode=null, psCode=null, advertisingLicenseCode=null, copyrightInformation=null, country=null, option=, provinceCode=null, provinceName=null, collectFlag=false), detailUrlCn=https://castjournals.cast.org.cn/joweb/bgkj/CN/Y2024/V50/I2/32, detailUrlEn=https://castjournals.cast.org.cn/joweb/bgkj/EN/Y2024/V50/I2/32, pdfUrlCn=https://castjournals.cast.org.cn/joweb/bgkj/CN/PDF/Y2024/V50/I2/32, pdfUrlEn=https://castjournals.cast.org.cn/joweb/bgkj/EN/PDF/Y2024/V50/I2/32, aliStartDate=null, aliEndDate=null, collectionFlag=false, citedCount=null, citedUrl=null, reference=null)
收藏切换
冷轧板SPCC开裂分析及改进
收藏切换
PDF下载
郭冬青 , 王少炳 , 黄利 , 杨雄
包钢科技 | 品种质量与试验研究 2024,50(2): 32-35
收起
收藏切换
包钢科技 | 品种质量与试验研究 2024, 50(2): 32-35
冷轧板SPCC开裂分析及改进
全屏
郭冬青, 王少炳, 黄利, 杨雄
作者信息
  • 内蒙古包钢钢联股份有限公司技术中心,内蒙古 包头 014010
  • 郭冬青(1988-),女,内蒙古乌兰察布市人,硕士,高级工程师,现从事板材新产品研发工作。

Analysis and Improvement on Cracking of Cold Rolled Sheet SPCC
Dong-qing Guo, Shao-bing Wang, Li Huang, Xiong Yang
Affiliations
  • Technical Center of Inner Mongolia Baotou Steel Union Co., Ltd., Baotou 014010, Inner Mongolia Autonomous Region, China
出版时间: 2024-04-25
文章导航
收藏切换

2 250 mm生产线生产的冷轧基料SPCC冷轧退火后的冷轧板,用户反映其成品延伸率低,在冲压成型过程中旋压部位不易成型,开裂率较高。针对此种情况进行原因分析,2 250 mm生产线生产的冷轧钢带SPCC Mn元素含量高是造成钢带强度略高的原因之一,钢带强度高,延伸率低,钢带易开裂;两条生产线冷却模式不同,2 250 mm生产线采用前集中冷却模式,CSP生产线采用前分散冷却模式,采用前集中冷却模式会造成热轧钢带强度略高,延伸率低,钢带易开裂。对应3.0~5.0 mm厚原料2 250 mm生产线生产的热轧钢带延伸率低于CSP生产线生产的热轧钢带,由于轧制的“遗传性”,热轧钢带延伸率高一般经冷轧退火后冷轧钢带延伸率也略高。

CSP生产线  /  2 250 mm生产线  /  性能  /  工艺

The feedback of user is that the elongation of cold rolled sheet with cold rolled base material SPCC manufactured by 2 250 mm production line after cold rolling and annealing is low, part of flow forming is not easily to form in punch forming process and cracking rate is higher. The cause analysis showed that its high Mn content was one of the causes for slightly higher strength of steel strip so that elongation was low and steel strip was easy to crack; cooling modes of the two production lines were different, the cooling mode of preconcentration was adopted by 2 250 mm production line and the cooling mode of predispersion was adopted by CSP production line so that the strength of hot rolled steel strip manufactured by 2 250 mm production line was slightly higher, elongation was low and steel strip was easy to crack. The elongation of hot rolled steel strip manufactured with raw materials with thickness of 3.0~5.0 mm by 2 250 mm production line is lower than that of hot rolled steel strip manufactured by CSP production line so that the elongation of cold rolled steel strip after cold rolling and annealing is also slightly higher due to the “heredity” of rolling.

CSP production line  /  2 250 mm production line  /  property  /  technology
郭冬青, 王少炳, 黄利, 杨雄. 冷轧板SPCC开裂分析及改进. 包钢科技, 2024 , 50 (2) : 32 -35 .
Dong-qing Guo, Shao-bing Wang, Li Huang, Xiong Yang. Analysis and Improvement on Cracking of Cold Rolled Sheet SPCC[J]. Science & Technology of Baotou Steel, 2024 , 50 (2) : 32 -35 .
一般用冷轧碳钢钢板或钢带SPCC主要是通过热轧钢带经过冷轧工艺生产,其表面光滑干净,主要用在汽车零部件或家用电器。冷轧板SPCC要求具有良好的冲压成型性能,但是冲压过程中的开裂对用户生产效率带来不利的影响,因此冷轧板SPCC开裂研究很重要。
2 250 mm热轧生产线生产的冷轧基料SPCC经1 750 mm冷轧生产线罩式退火后冷轧板供用户使用过程中,用户反映钢板延伸率低,在冲压成型过程中旋压部位不易成型,开裂率高,短流程CSP生产线生产的冷轧基料SPCC经冷轧罩式退火后冷轧板开裂率低。开裂发生在旋压变形位置,此处钢带最薄,强度最高,本身是开裂风险最大的区域,所以要求塑性最低处金属必须具有高的延伸率。延伸率是影响成型性能的关键因素,板带延伸率低容易开裂,开裂倾向明显。分别对供用户厚度规格为0.8 mm、1.0 mm、1.2 mm、1.5 mm、1.8 mm、2.0 mm、2.5 mm、3.0 mm的冷轧板抗拉强度、屈服强度、延伸率、屈强比数值经统计作平均值处理后对比图见图1,可以看出2 250 mm生产线冷轧基料生产的SPCC冷轧板与CSP生产线冷轧基料生产的SPCC冷轧板抗拉强度、屈服强度相差不明显,厚度规格为0.8 mm、1.0 mm、1.5 mm、1.8 mm 2 250 mm生产线生产的冷轧板延伸率比CSP生产线生产的冷轧板延伸率略低。
2 250 mm生产线生产的SPCC冷轧基料与CSP生产线生产的SPCC冷轧基料化学成分平均值见表1。炼钢过程加强原料品质检查及严格控制化学成分,以减少夹杂物的产生[1]
对2 250 mm生产线生产的SPCC冷轧基料与CSP生产线生产的SPCC冷轧基料化学成分进行统计,其中对强度有贡献的元素C、Si含量平均值接近,2 250 mm生产线生产的SPCC冷轧基料Mn元素含量比CSP生产线约高0.05个百分点,Mn具有固溶强化的作用,可以提高钢的强度,扩大奥氏体相区,降低过冷奥氏体的相变温度,有利于细化铁素体晶粒[2-3],所以2 250 mm生产线生产的冷轧基料Mn元素含量高是造成钢板强度略高的原因之一,一般钢板强度高,延伸率低,钢板易开裂。
为保证低碳钢冷轧成品的冲压性能,国内外的研究和生产实践都表明[4-5]在热轧时应采用“三高一低”制度,即高的加热温度、开轧温度和终轧温度及低的卷取温度,避免进入两相区轧制,以得到均匀细小的热轧态晶粒,并且阻止AlN在卷取时析出,使AlN在退火时先析出,促使晶粒择优取向,形成强的{111}织构[6]
轧制冷却过程中要控制合适的终轧温度,加速冷却以加速相变的过程,所以合理的终轧温度和冷却方式是热轧低碳钢得到理想铁素体组织的关键。2 250 mm与CSP生产线热轧轧制工艺比较见表2,2 250 mm生产线与CSP生产线的主要工艺设计不同,其一是热轧温度控制精度不同,2 250 mm生产线卷取温度薄规格为600±15 ℃,厚规格为580±15 ℃,而CSP生产线按厚度组距更细化,比2 250 mm生产线低10 ℃;其二是冷却模式不同,2 250 mm生产线采用前集中冷却模式,CSP生产线采用前分散冷却模式,采用前集中冷却模式会造成热轧钢带强度略高,延伸率略低,是造成2 250 mm生产线生产的冷轧钢板易于开裂的工艺因素之一。
对供用户的2 250 mm生产线生产的SPCC冷轧基料与CSP生产线生产的SPCC冷轧基料抗拉强度、屈服强度、延伸率、屈强比数值经统计作平均值处理后对比见图2
可以看出2 250 mm生产线生产的薄规格SPCC冷轧基料比CSP生产线生产的薄规格SPCC冷轧基料抗拉强度略高,高约5~6 MPa;而2 250 mm生产线生产的规格为3.0~5.0 mm基料的延伸率均比CSP生产线生产的基料低,由于热轧“遗传性”,冷轧基料延伸率低,热轧钢带经后续冷轧、退火后冷轧钢板延伸率也偏低,这也是造成2 250 mm生产线生产的冷轧板在冲压过程中比CSP生产线生产的冷轧板延伸率偏低的原因。
调整2 250 mm生产线生产冷轧基料SPCC Mn元素含量,Mn含量控制在0.10%~0.15%。降低轧制后冷却能力,热轧层流冷却方式采用隔一开一的前分散冷却模式。通过采取上述控制措施提高了薄规格冷轧钢带延伸率。
通过优化化学成分及降低轧后冷却能力提高了冷轧钢带SPCC延伸率,大大减小了钢带开裂率,为下游用户深加工提供了良好的原材料,提高了用户的生产效率。
参考文献 引证文献
排序方式:
[1]
汪凤, 范玉然, 尹长华, 等. Q235B钢板冷弯开裂原因分析[J]. 金属热处理, 2011, 34(S1):158-160.
[2]
张中平. 高强汽车大梁钢微观组织控制与TMCP工艺开发[D]. 沈阳: 东北大学, 2007.
[3]
刘跃飞. Q345B热轧钢板加工开裂的原因分析[J]. 金属材料与冶金工程, 2015, 43(1):21-23.
[4]
许洪新. 汽车用钢研究开发的现状和发展[J]. 太钢科技, 1996(4):1-9.
[5]
李明久. 08Al冷板性能升级的开发研究[J]. 鞍钢技术, 1991(3):13-16.
[6]
常军, 张开华, 程兴德, 等. 终轧温度和卷取温度对低碳铝镇静钢性能的影响[J]. 钢铁钒钛, 1991(3):13-16.
2024年第50卷第2期
PDF下载
173
81
引用本文
BibTeX
文章信息
  • 接收时间:2024-01-28
  • 首发时间:2025-10-23
  • 出版时间:2024-04-25
补充材料
相关文章
文章信息
作者
出版历史
  • 收稿日期:2024-01-28
基金
作者信息
    内蒙古包钢钢联股份有限公司技术中心,内蒙古 包头 014010
参考文献
分享链接
https://castjournals.cast.org.cn/joweb/bgkj/CN/1188049105763840093
分享至
全文二维码

扫描看全文

引用本文
BibTeX
本文的引用情况
2种不同金属材料的力学参数

Family
属数
Number of
genus
种数
Number of
species
占总种数比例
Percentage of
total species (%)

Genus
种数
Number of
species
占总种数比例
Percentage of total
species (%)
鹅膏菌科Amanitaceae 2 11 5.26 鹅膏菌属 Amanita 10 4.78
小菇科 Mycenaceae 2 12 5.74 丝盖伞属 Inocybe 5 2.39
多孔菌科 Polyporaceae 8 14 6.70 蜡蘑属 Laccaria 5 2.39
红菇科 Russulaceae 3 23 11.00 小皮伞属 Marasmius 6 2.87
小菇属 Mycena 11 5.26
光柄菇属 Pluteus 5 2.39
红菇属 Russula 17 8.13
栓菌属 Trametes 5 2.39
关闭全屏