Article(id=1327335883793085341, tenantId=1146029695717560320, journalId=1319355204128309394, issueId=1327335794341163146, articleNumber=null, orderNo=null, doi=10.3969/j.issn.1001-4837.2025.11.002, pmid=null, cstr=null, oa=null, hot=null, price=null, onlineType=0, articleFormat=0, articleType=null, articleTypeStr=null, receivedDate=1758470400000, receivedDateStr=2025-09-22, revisedDate=1761148800000, revisedDateStr=2025-10-23, acceptedDate=null, acceptedDateStr=null, onlineDate=1794391135403, onlineDateStr=2026-11-11, pubDate=1764432000000, pubDateStr=2025-11-30, doiRegisterDate=null, doiRegisterDateStr=null, onlineIssueDate=1794391135403, onlineIssueDateStr=2026-11-11, onlineJustAcceptDate=null, onlineJustAcceptDateStr=null, onlineFirstDate=null, onlineFirstDateStr=null, sourceXml=null, magXml=null, createTime=1794391135403, creator=13701087609, updateTime=1794391135403, updator=13701087609, issue=Issue{id=1327335794341163146, tenantId=1146029695717560320, journalId=1319355204128309394, year='2025', volume='42', issue='11', pageStart='1', pageEnd='86', issueExtLink='null', onlineDate='null', pubDate='1764432000000', pubDateStr='2025-11-30', beforeIssueId=null, nextIssueId=null, price=null, status=1, issueComplete=1, articleOrder=1, issueType=-1, specialIssue=null, createTime=1794391114077, creator='13701087609', updateTime=1794452638835, updator='13701087609', preIssue=null, nextIssue=null, articleTotal=null, ext={EN=IssueExt(id=1327593848248841181, tenantId=1146029695717560320, journalId=1319355204128309394, issueId=1327335794341163146, language=EN, specialIssueTitle=, coverIllustrator=null, specialIssueEditor=, specialIssueAbout=), CN=IssueExt(id=1327593848248841182, tenantId=1146029695717560320, journalId=1319355204128309394, issueId=1327335794341163146, language=CN, specialIssueTitle=, coverIllustrator=null, specialIssueEditor=, specialIssueAbout=)}, issueFiles=null, downloadFileDto=null}, startPage=11, endPage=22, ext={EN=ArticleExt(id=1327335884006994846, articleId=1327335883793085341, tenantId=1146029695717560320, journalId=1319355204128309394, language=EN, title=Industrial application research of domestic welding materials for main weld seams of 12Cr2Mo1V steel hydrotreating reactors, columnId=1320422992476226524, journalTitle=Pressure Vessel Technology, columnName=Experimental Researches, runingTitle=null, highlight=null, articleAbstract=

To address the issues of long procurement cycles and high costs caused by long term reliance on imported welding materials for the main weld seams of 12Cr2Mo1V steel hydrotreating reactors,a solution is proposed that involves adopting domestic welding materials and conducting systematic welding tests in accordance with NB/T 47014—2023 Welding procedure qualification for pressure equipments.The results show that the properties of the domestic welded joints,including tensile strength,impact toughness,bending performance,temper embrittlement susceptibility,and high temperature creep resistance,all meet equipment manufacturing requirements,reaching the level of similar imported products,with some data being even better.These welding materials have been successfully applied to the manufacturing of main weld seams in multiple reactors,achieving industrial application.The study provides practical evidence and references for advancing the localization of such high end welding materials,reducing manufacturing costs,and shortening delivery cycles.

, authors=Chenglin WU1, Min WAN1, Taiping GUO1, Yingjun WANG1, Chenggang CHU2, Xuejiao WANG1, authorsList=Chenglin WU, Min WAN, Taiping GUO, Yingjun WANG, Chenggang CHU, Xuejiao WANG, authorCompany=null, correspAuthors=null, authorNote=null, correspAuthorsNote=null, copyrightStatement=null, copyrightOwner=null, extLink=null, articleAbsUrl=null, sourceXml=null, magXml=null, pdfUrl=null, pdf=null, pdfFileSize=null, pdfExtLink=null, richHtmlUrl=null, mobilePdfUrl=null, reviewReport=null, pdfFirstPage=null, abstractGraph=null, abstractGraphContent=null, abstractVideo=null, citation=null, cebUrl=null, magXmlContent=null, mapNumber=null, fund=null), CN=ArticleExt(id=1327335887538598837, articleId=1327335883793085341, tenantId=1146029695717560320, journalId=1319355204128309394, language=CN, title=12Cr2Mo1V钢制加氢反应器主焊缝国产焊材工业化应用研究, columnId=1320422992698524638, journalTitle=压力容器, columnName=试验研究, runingTitle=null, highlight=null, articleAbstract=

针对12Cr2Mo1V钢加氢反应器主焊缝焊接材料长期依赖进口导致的采购周期长、成本高的问题,提出采用国产焊材替代并依据NB/T 47014—2023《承压设备焊接工艺评定》开展系统焊接试验的解决方案。结果表明,国产焊接接头的拉伸、冲击、弯曲、回火脆化倾向及高温蠕变等性能均满足设备制造要求,达到同类进口产品水平,部分数据更优。该焊材已成功应用于多台反应器主焊缝制造,实现了工业化应用。研究为推进该类高端焊接材料国产化、降低制造成本与缩短交付周期提供了实践依据与参考。

, authors=吴成林1, 万敏1, 郭太平1, 王迎君1, 楚成刚2, 王雪骄1, authorsList=吴成林, 万敏, 郭太平, 王迎君, 楚成刚, 王雪骄, authorCompany=null, correspAuthors=null, authorNote=

吴成林(1988),男,高级工程师,主要从事核电与压力容器焊接工艺技术工作,通信地址:618000四川省德阳市旌阳区珠江西路460号二重(德阳)重型装备有限公司核电石化公司核容所,E-mail:。

, correspAuthorsNote=null, copyrightStatement=作者向本刊所投稿件一经本刊录用,则该论文的复制权、发行权、信息网络传播权、翻译权、汇编权等权利视为自动转让给本刊。本刊为国内各主要数据库收录期刊,本刊所发表的稿件将同时通过因特网进行网络出版或提供信息服务(包括印刷版、光盘版和网络版等各种使用方式)。, copyrightOwner=null, extLink=null, articleAbsUrl=null, sourceXml=XKkVrkC+B6KBCMD2It2J1A==, magXml=vNRCxtfzCPrSOkiaJVcaMA==, pdfUrl=null, pdf=tQAxJh1Xr8pDRNk3cSfIIA==, pdfFileSize=22383689, pdfExtLink=null, richHtmlUrl=null, mobilePdfUrl=null, reviewReport=null, pdfFirstPage=null, abstractGraph=U7kfPwSk2a+gUqapxSSHXg==, abstractGraphContent=null, abstractVideo=null, citation=null, cebUrl=null, magXmlContent=XFsl6jr767Jl6V6IMJWMCw==, mapNumber=null, fund=null)}, authors=[Author(id=1327335887920280509, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, orderNo=0, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=908499928@qq.com, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335887995777983, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335887920280509, language=EN, stringName=Chenglin WU, firstName=Chenglin, middleName=null, lastName=WU, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335888075469760, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335887920280509, language=CN, stringName=吴成林, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1二重(德阳)重型装备有限公司,四川 德阳 618000, bio={"content":"

吴成林(1988),男,高级工程师,主要从事核电与压力容器焊接工艺技术工作,通信地址:618000四川省德阳市旌阳区珠江西路460号二重(德阳)重型装备有限公司核电石化公司核容所,E-mail:。

"}, bioImg=null, bioContent=

吴成林(1988),男,高级工程师,主要从事核电与压力容器焊接工艺技术工作,通信地址:618000四川省德阳市旌阳区珠江西路460号二重(德阳)重型装备有限公司核电石化公司核容所,E-mail:。

, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335887752508342, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, xref=1, ext=[AuthorCompanyExt(id=1327335887760896951, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China), AuthorCompanyExt(id=1327335887769285560, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1二重(德阳)重型装备有限公司,四川 德阳 618000)])]), Author(id=1327335888146772930, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, orderNo=1, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335888213881796, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335888146772930, language=EN, stringName=Min WAN, firstName=Min, middleName=null, lastName=WAN, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335888272602053, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335888146772930, language=CN, stringName=万敏, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1二重(德阳)重型装备有限公司,四川 德阳 618000, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335887752508342, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, xref=1, ext=[AuthorCompanyExt(id=1327335887760896951, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China), AuthorCompanyExt(id=1327335887769285560, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1二重(德阳)重型装备有限公司,四川 德阳 618000)])]), Author(id=1327335888348099527, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, orderNo=2, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335888440374217, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335888348099527, language=EN, stringName=Taiping GUO, firstName=Taiping, middleName=null, lastName=GUO, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335888503288778, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335888348099527, language=CN, stringName=郭太平, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1二重(德阳)重型装备有限公司,四川 德阳 618000, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335887752508342, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, xref=1, ext=[AuthorCompanyExt(id=1327335887760896951, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China), AuthorCompanyExt(id=1327335887769285560, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1二重(德阳)重型装备有限公司,四川 德阳 618000)])]), Author(id=1327335888562009036, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, orderNo=3, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335888637506510, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335888562009036, language=EN, stringName=Yingjun WANG, firstName=Yingjun, middleName=null, lastName=WANG, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335888704615375, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335888562009036, language=CN, stringName=王迎君, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1二重(德阳)重型装备有限公司,四川 德阳 618000, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335887752508342, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, xref=1, ext=[AuthorCompanyExt(id=1327335887760896951, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China), AuthorCompanyExt(id=1327335887769285560, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1二重(德阳)重型装备有限公司,四川 德阳 618000)])]), Author(id=1327335890403308497, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, orderNo=4, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335890483000275, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335890403308497, language=EN, stringName=Chenggang CHU, firstName=Chenggang, middleName=null, lastName=CHU, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=2, address=2Sichuan Xiye New Material Co.,Ltd.,Chengdu 610000,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335890550109140, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335890403308497, language=CN, stringName=楚成刚, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=2, address=2四川西冶新材料股份有限公司,成都 610000, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335887836394425, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, xref=2, ext=[AuthorCompanyExt(id=1327335887848977338, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887836394425, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=2Sichuan Xiye New Material Co.,Ltd.,Chengdu 610000,China), AuthorCompanyExt(id=1327335887853171643, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887836394425, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=2四川西冶新材料股份有限公司,成都 610000)])]), Author(id=1327335890604635094, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, orderNo=5, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335890680132568, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335890604635094, language=EN, stringName=Xuejiao WANG, firstName=Xuejiao, middleName=null, lastName=WANG, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335890751435737, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335890604635094, language=CN, stringName=王雪骄, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1二重(德阳)重型装备有限公司,四川 德阳 618000, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335887752508342, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, xref=1, ext=[AuthorCompanyExt(id=1327335887760896951, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China), AuthorCompanyExt(id=1327335887769285560, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1二重(德阳)重型装备有限公司,四川 德阳 618000)])])], keywords=[Keyword(id=1327335890843710426, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, orderNo=1, keyword=12Cr2Mo1V steel), Keyword(id=1327335890906624987, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, orderNo=2, keyword=hydrotreating reactor), Keyword(id=1327335890969539548, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, orderNo=3, keyword=localization of welding materials), Keyword(id=1327335891028259805, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, orderNo=4, keyword=industrial application), Keyword(id=1327335891082785758, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, orderNo=1, keyword=12Cr2Mo1V钢), Keyword(id=1327335891137311711, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, orderNo=2, keyword=加氢反应器), Keyword(id=1327335891208614880, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, orderNo=3, keyword=焊材国产化), Keyword(id=1327335891284112354, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, orderNo=4, keyword=工业化应用)], refs=[Reference(id=1327335897613316123, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2020, volume=null, issue=6, pageStart=19, pageEnd=24, url=null, language=null, rfNumber=1, rfOrder=0, authorNames=蒋军, 房务农, journalName=金属加工(热加工), refType=null, unstructuredReference=蒋军,房务农.我国压力容器用高端焊接材料国产化现状及发展趋势[J].金属加工(热加工),2020(6):19-24., articleTitle=我国压力容器用高端焊接材料国产化现状及发展趋势, refAbstract=null), Reference(id=1327335897672036380, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2020, volume=null, issue=6, pageStart=19, pageEnd=24, url=null, language=null, rfNumber=1, rfOrder=1, authorNames=JIANG J, FANG W N, journalName=MW Metal Forming, refType=null, unstructuredReference=JIANG J,FANG W N.Current status and development trend of localization of high‑end welding materials for pressure vessels[J].MW Metal Forming,2020(6):19-24., articleTitle=Current status and development trend of localization of high‑end welding materials for pressure vessels, refAbstract=null), Reference(id=1327335899349757982, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2, volume=31, issue=12, pageStart=73, pageEnd=78, url=null, language=null, rfNumber=2, rfOrder=2, authorNames=张颖, 尚尔晶, 谷文, journalName=Cr-1Mo和2.25Cr-1Mo-0, refType=null, unstructuredReference=张颖,尚尔晶,谷文.2.25Cr-1Mo和2.25Cr-1Mo-0.25V钢加氢反应器材料和制造经验[J].压力容器,2014,31(12):73-78., articleTitle=25, refAbstract=null), Reference(id=1327335899433644063, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2014, volume=31, issue=12, pageStart=73, pageEnd=78, url=null, language=null, rfNumber=2, rfOrder=3, authorNames=ZHANG Y, SHANG E J, GU W, journalName=Pressure Vessel Technology, refType=null, unstructuredReference=ZHANG Y,SHANG E J,GU W.Materials and fabrication experience of 2.25Cr-1Mo and 2.25Cr-1Mo-0.25V steel hydrogenation reactor[J].Pressure Vessel Technology,2014,31(12):73-78., articleTitle=Materials and fabrication experience of 2.25Cr-1Mo and 2.25Cr-1Mo-0.25V steel hydrogenation reactor, refAbstract=null), Reference(id=1327335899534307360, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2009, volume=30, issue=1, pageStart=28, pageEnd=31, url=null, language=null, rfNumber=3, rfOrder=4, authorNames=陈晓玲, 李多民, 段滋华, journalName=化工装备技术, refType=null, unstructuredReference=陈晓玲,李多民,段滋华.加氢反应器的发展现状[J].化工装备技术,2009,30(1):28-31., articleTitle=加氢反应器的发展现状, refAbstract=null), Reference(id=1327335899618193441, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2009, volume=30, issue=1, pageStart=28, pageEnd=31, url=null, language=null, rfNumber=3, rfOrder=5, authorNames=CHEN X L, LI D M, DUAN Z H, journalName=Chemical Equipment Technology, refType=null, unstructuredReference=CHEN X L,LI D M,DUAN Z H.Development status of hydrogenation reactor[J].Chemical Equipment Technology,2009,30(1):28-31., articleTitle=Development status of hydrogenation reactor, refAbstract=null), Reference(id=1327335899702079522, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2023, volume=null, issue=5, pageStart=32, pageEnd=36, url=null, language=null, rfNumber=4, rfOrder=6, authorNames=王雪骄, 范阳阳, 晏君文, journalName=大型铸锻件, refType=null, unstructuredReference=王雪骄,范阳阳,晏君文,等.2.25Cr-1Mo-0.25V钢上国产焊材单层带极堆焊工艺研究[J].大型铸锻件,2023(5):32-36., articleTitle=2.25Cr-1Mo-0.25V钢上国产焊材单层带极堆焊工艺研究, refAbstract=null), Reference(id=1327335899781771299, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2023, volume=null, issue=5, pageStart=32, pageEnd=36, url=null, language=null, rfNumber=4, rfOrder=7, authorNames=WANG X J, FAN Y Y, YAN J W, journalName=Heavy Casting and Forging, refType=null, unstructuredReference=WANG X J,FAN Y Y,YAN J W,et al.Research on the technology of single‑layered strip surfacing on 2.25Cr-1Mo-0.25V steel with domestic welding materials[J].Heavy Casting and Forging,2023(5):32-36., articleTitle=Research on the technology of single‑layered strip surfacing on 2.25Cr-1Mo-0.25V steel with domestic welding materials, refAbstract=null), Reference(id=1327335899861463076, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2, volume=null, issue=null, pageStart=null, pageEnd=null, url=null, language=null, rfNumber=5, rfOrder=8, authorNames=王小刚, journalName=Cr-1Mo-0, refType=null, unstructuredReference=王小刚.2.25Cr-1Mo-0.25V钢埋弧焊焊材及熔敷金属组织性能研究[D].北京:机械科学研究总院,2006., articleTitle=25, refAbstract=null), Reference(id=1327335899924377637, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2006, volume=null, issue=null, pageStart=null, pageEnd=null, url=null, language=null, rfNumber=5, rfOrder=9, authorNames=WANG X G, journalName=null, refType=null, unstructuredReference=WANG X G.Study on the submerged arc welding consumables for 2.25Cr-1Mo-0.25V steel and its microstructure and mechanical properties of the deposited metal[D].Beijing:Academy of Machinery Science & Technology,2006., articleTitle=Study on the submerged arc welding consumables for 2.25Cr-1Mo-0, refAbstract=null), Reference(id=1327335899983097894, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=1993, volume=null, issue=4, pageStart=268, pageEnd=272, url=null, language=null, rfNumber=6, rfOrder=10, authorNames=魏艳红, 张修智, 杜文, journalName=焊接学报, refType=null, unstructuredReference=魏艳红,张修智,杜文,等.焊接接头机械性能预测专家系统——PPES[J].焊接学报,1993(4):268-272., articleTitle=焊接接头机械性能预测专家系统——PPES, refAbstract=null), Reference(id=1327335900054401063, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=1993, volume=null, issue=4, pageStart=268, pageEnd=272, url=null, language=null, rfNumber=6, rfOrder=11, authorNames=WEI Y H, ZHANG X Z, DU W, journalName=Transactions of the China Welding Institution, refType=null, unstructuredReference=WEI Y H,ZHANG X Z,DU W,et al.Expert system for predicting mechanical properties of welded joints—PPES[J].Transactions of the China Welding Institution,1993(4):268-272., articleTitle=Expert system for predicting mechanical properties of welded joints—PPES, refAbstract=null), Reference(id=1327335900113121320, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2002, volume=null, issue=3, pageStart=75, pageEnd=79, url=null, language=null, rfNumber=7, rfOrder=12, authorNames=汪建华, 陆皓, journalName=焊接学报, refType=null, unstructuredReference=汪建华,陆皓.焊接残余应力形成机制与消除原理若干问题的讨论[J].焊接学报,2002(3):75-79., articleTitle=焊接残余应力形成机制与消除原理若干问题的讨论, refAbstract=null), Reference(id=1327335900192813097, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2002, volume=null, issue=3, pageStart=75, pageEnd=79, url=null, language=null, rfNumber=7, rfOrder=13, authorNames=WANG J H, LU H, journalName=Transactions of the China Welding Institution, refType=null, unstructuredReference=WANG J H,LU H.Some discussions on principle of causing and relieving welding residual stress[J].Transactions of the China Welding Institution,2002(3):75-79., articleTitle=Some discussions on principle of causing and relieving welding residual stress, refAbstract=null), Reference(id=1327335900268310570, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2, volume=21, issue=10, pageStart=10, pageEnd=13, url=null, language=null, rfNumber=8, rfOrder=14, authorNames=薛巍, 李南, 党兆凯, journalName=Cr-1Mo-0, refType=null, unstructuredReference=薛巍,李南,党兆凯.2.25Cr-1Mo-0.25V钢板热处理工艺试验[J].压力容器,2004,21(10):10-13., articleTitle=25, refAbstract=null), Reference(id=1327335900343808043, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2004, volume=21, issue=10, pageStart=10, pageEnd=13, url=null, language=null, rfNumber=8, rfOrder=15, authorNames=XUE W, LI N, DANG Z K, journalName=Pressure Vessel Technology, refType=null, unstructuredReference=XUE W,LI N,DANG Z K.Test on heat treatment of 2.25Cr-1Mo-0.25V steel plate[J].Pressure Vessel Technology,2004,21(10):10-13., articleTitle=Test on heat treatment of 2.25Cr-1Mo-0.25V steel plate, refAbstract=null), Reference(id=1327335900406722604, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2016, volume=40, issue=2, pageStart=98, pageEnd=101, url=null, language=null, rfNumber=9, rfOrder=16, authorNames=张敏, 徐蔼彦, 汪强, journalName=机械工程材料, refType=null, unstructuredReference=张敏,徐蔼彦,汪强,等.高温运行后12Cr1MoV钢焊接接头的显微组织和力学性能[J].机械工程材料,2016,40(2):98-101., articleTitle=高温运行后12Cr1MoV钢焊接接头的显微组织和力学性能, refAbstract=null), Reference(id=1327335900465442861, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2016, volume=40, issue=2, pageStart=98, pageEnd=101, url=null, language=null, rfNumber=9, rfOrder=17, authorNames=ZHANG M, XU A Y, WANG Q, journalName=Materials for Mechanical Engineering, refType=null, unstructuredReference=ZHANG M,XU A Y,WANG Q,et al.Microstructure and mechanical properties of 12Cr1MoV steel welded joint after high temperature service[J].Materials for Mechanical Engineering,2016,40(2):98-101., articleTitle=Microstructure and mechanical properties of 12Cr1MoV steel welded joint after high temperature service, refAbstract=null), Reference(id=1327335900645797934, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2020, volume=38, issue=4, pageStart=625, pageEnd=628, url=null, language=null, rfNumber=10, rfOrder=18, authorNames=马窦琴, 宋亚虎, 赵学谦, journalName=材料科学与工程学报, refType=null, unstructuredReference=马窦琴,宋亚虎,赵学谦,等.加氢锻件用2.25Cr-1Mo-0.25V钢的冲击韧性[J].材料科学与工程学报,2020,38(4):625-628., articleTitle=加氢锻件用2.25Cr-1Mo-0.25V钢的冲击韧性, refAbstract=null), Reference(id=1327335900729684015, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2020, volume=38, issue=4, pageStart=625, pageEnd=628, url=null, language=null, rfNumber=10, rfOrder=19, authorNames=MA D Q, SONG Y H, ZHAO X Q, journalName=Journal of Materials Science and Engineering, refType=null, unstructuredReference=MA D Q,SONG Y H,ZHAO X Q,et al.Research on impact toughness of 2.25Cr-1Mo-0.25V steel for hydrogenation forgings[J].Journal of Materials Science and Engineering,2020,38(4):625-628., articleTitle=Research on impact toughness of 2.25Cr-1Mo-0.25V steel for hydrogenation forgings, refAbstract=null), Reference(id=1327335900796792880, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2019, volume=39, issue=5, pageStart=60, pageEnd=61, url=null, language=null, rfNumber=11, rfOrder=20, authorNames=柯杨, 刘仕伟, journalName=冶金与材料, refType=null, unstructuredReference=柯杨,刘仕伟.压力容器材料韧脆转变温度曲线拟合分析及应用研究[J].冶金与材料,2019,39(5):60-61., articleTitle=压力容器材料韧脆转变温度曲线拟合分析及应用研究, refAbstract=null), Reference(id=1327335900859707441, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2019, volume=39, issue=5, pageStart=60, pageEnd=61, url=null, language=null, rfNumber=11, rfOrder=21, authorNames=KE Y, LIU S W, journalName=Metallurgy and Materials, refType=null, unstructuredReference=KE Y,LIU S W.Curve fitting analysis and application research on ductile-brittle transition temperature of pressure vessel materials[J].Metallurgy and Materials,2019,39(5):60-61., articleTitle=Curve fitting analysis and application research on ductile-brittle transition temperature of pressure vessel materials, refAbstract=null), Reference(id=1327335900935204914, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2020, volume=37, issue=2, pageStart=1, pageEnd=10, url=null, language=null, rfNumber=12, rfOrder=22, authorNames=马韩韩, 伏玮, 沈志鹏, journalName=压力容器, refType=null, unstructuredReference=马韩韩,伏玮,沈志鹏,等.基于步冷试验的2.25Cr-1Mo-0.25V钢母材及焊缝回火脆化研究[J].压力容器,2020,37(2):1-10., articleTitle=基于步冷试验的2.25Cr-1Mo-0.25V钢母材及焊缝回火脆化研究, refAbstract=null), Reference(id=1327335901006508083, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2020, volume=37, issue=2, pageStart=1, pageEnd=10, url=null, language=null, rfNumber=12, rfOrder=23, authorNames=MA H H, FU W, SHEN Z P, journalName=Pressure Vessel Technology, refType=null, unstructuredReference=MA H H,FU W,SHEN Z P,et al.Study on temper embrittlement of 2.25Cr-1Mo-0.25V steel base metal and welded joint based on step‑cooling test[J].Pressure Vessel Technology,2020,37(2):1-10., articleTitle=Study on temper embrittlement of 2.25Cr-1Mo-0.25V steel base metal and welded joint based on step‑cooling test, refAbstract=null), Reference(id=1327335901094588468, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2015, volume=null, issue=null, pageStart=null, pageEnd=null, url=null, language=null, rfNumber=13, rfOrder=24, authorNames=张敬强, journalName=null, refType=null, unstructuredReference=张敬强.焊接接头中应力促进氢致裂纹形成理论分析与实验研究[D].哈尔滨:哈尔滨工业大学,2015., articleTitle=焊接接头中应力促进氢致裂纹形成理论分析与实验研究, refAbstract=null), Reference(id=1327335901170085941, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2015, volume=null, issue=null, pageStart=null, pageEnd=null, url=null, language=null, rfNumber=13, rfOrder=25, authorNames=ZHANG J Q, journalName=null, refType=null, unstructuredReference=ZHANG J Q.Theoretical analysis and experimental research on stress‑facilitated nucleation of hydrogen induced cracking in welded joint[D].Harbin:Harbin Institute of Technology,2015., articleTitle=Theoretical analysis and experimental research on stress‑facilitated nucleation of hydrogen induced cracking in welded joint, refAbstract=null), Reference(id=1327335901237194806, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2017, volume=53, issue=12, pageStart=879, pageEnd=881, url=null, language=null, rfNumber=14, rfOrder=26, authorNames=宗杰, 蒋志强, journalName=理化检验(物理分册), refType=null, unstructuredReference=宗杰,蒋志强.熔敷金属中扩散氢含量的测定[J].理化检验(物理分册),2017,53(12):879-881., articleTitle=熔敷金属中扩散氢含量的测定, refAbstract=null), Reference(id=1327335901300109367, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2017, volume=53, issue=12, pageStart=879, pageEnd=881, url=null, language=null, rfNumber=14, rfOrder=27, authorNames=ZONG J, JIANG Z Q, journalName=Physical Testing and Chemical Analysis(Part A:Physical Testing), refType=null, unstructuredReference=ZONG J,JIANG Z Q.Determination of diffusible hydrogen content in deposited metals[J].Physical Testing and Chemical Analysis(Part A:Physical Testing),2017,53(12):879-881., articleTitle=Determination of diffusible hydrogen content in deposited metals, refAbstract=null), Reference(id=1327335901367218232, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2, volume=null, issue=null, pageStart=null, pageEnd=null, url=null, language=null, rfNumber=15, rfOrder=28, authorNames=武欣宇, journalName=null, refType=null, unstructuredReference=武欣宇.2.25Cr1MoV钢加氢反应设备蠕变疲劳寿命设计方法[D].天津:天津大学,2015., articleTitle=25Cr1MoV钢加氢反应设备蠕变疲劳寿命设计方法, refAbstract=null), Reference(id=1327335901442715705, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2015, volume=null, issue=null, pageStart=null, pageEnd=null, url=null, language=null, rfNumber=15, rfOrder=29, authorNames=WU X Y, journalName=Tianjin:Tianjin University, refType=null, unstructuredReference=WU X Y.A design approach for creep fatigue evaluation of hydrogenation reactor made of 2.25Cr1MoV steel[J].Tianjin:Tianjin University,2015., articleTitle=A design approach for creep fatigue evaluation of hydrogenation reactor made of 2.25Cr1MoV steel, refAbstract=null), Reference(id=1327335901518213178, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2, volume=null, issue=null, pageStart=null, pageEnd=null, url=null, language=null, rfNumber=16, rfOrder=30, authorNames=韩一纯, journalName=null, refType=null, unstructuredReference=韩一纯.2.25Cr1Mo0.25V钢再热裂纹生成机理研究[D].合肥:中国科学技术大学,2015., articleTitle=25Cr1Mo0.25V钢再热裂纹生成机理研究, refAbstract=null), Reference(id=1327335901581127739, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2015, volume=null, issue=null, pageStart=null, pageEnd=null, url=null, language=null, rfNumber=16, rfOrder=31, authorNames=HAN Y C, journalName=null, refType=null, unstructuredReference=HAN Y C.Study on the mechanism of reheat cracking in 2.25Cr1Mo0.25V steel[D].Hefei:University of Science and Technology of China,2015., articleTitle=Study on the mechanism of reheat cracking in 2.25Cr1Mo0.25V steel, refAbstract=null), Reference(id=1327335901652430908, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2019, volume=36, issue=11, pageStart=1, pageEnd=5, url=null, language=null, rfNumber=17, rfOrder=32, authorNames=卜华全, 任明皓, 姜恒, journalName=压力容器, refType=null, unstructuredReference=卜华全,任明皓,姜恒.Gleeble试验中再热裂纹敏感性评价方法探讨[J].压力容器,2019,36(11):1-5., articleTitle=Gleeble试验中再热裂纹敏感性评价方法探讨, refAbstract=null), Reference(id=1327335901719539773, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2019, volume=36, issue=11, pageStart=1, pageEnd=5, url=null, language=null, rfNumber=17, rfOrder=33, authorNames=BO H Q, REN M H, JIANG H, journalName=Pressure Vessel Technology, refType=null, unstructuredReference=BO H Q,REN M H,JIANG H.Discussion on evaluation method of reheat crack sensitivity in gleeble test[J].Pressure Vessel Technology,2019,36(11):1-5., articleTitle=Discussion on evaluation method of reheat crack sensitivity in gleeble test, refAbstract=null), Reference(id=1327335901803425854, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2024, volume=41, issue=4, pageStart=16, pageEnd=21, url=null, language=null, rfNumber=18, rfOrder=34, authorNames=王雪骄, 何鹏, 晏君文, journalName=压力容器, refType=null, unstructuredReference=王雪骄,何鹏,晏君文,等.12Cr2Mo1V钢凸台附加填充丝埋弧堆焊工艺研究[J]. 压力容器,2024,41(4):16-21., articleTitle=12Cr2Mo1V钢凸台附加填充丝埋弧堆焊工艺研究, refAbstract=null), Reference(id=1327335901874729023, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2024, volume=41, issue=4, pageStart=16, pageEnd=21, url=null, language=null, rfNumber=18, rfOrder=35, authorNames=WANG X J, HE P, YAN J W, journalName=Pressure Vessel Technology, refType=null, unstructuredReference=WANG X J,HE P,YAN J W,et al.Research of submerged arc welding build up technology of 12Cr2Mo1V steel boss using additional filing wire[J].Pressure Vessel Technology,2024,41(4):16-21., articleTitle=Research of submerged arc welding build up technology of 12Cr2Mo1V steel boss using additional filing wire, refAbstract=null), Reference(id=1327335901950226496, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2022, volume=39, issue=3, pageStart=9, pageEnd=18, url=null, language=null, rfNumber=19, rfOrder=36, authorNames=秦牧, 程光旭, 李青, journalName=压力容器, refType=null, unstructuredReference=秦牧,程光旭,李青,等.2.25Cr-1Mo-0.25V钢加氢反应器焊接接头的性能影响因素研究[J].压力容器,2022,39(3):9-18., articleTitle=2.25Cr-1Mo-0.25V钢加氢反应器焊接接头的性能影响因素研究, refAbstract=null), Reference(id=1327335902042501185, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, doi=null, pmid=null, pmcid=null, year=2022, volume=39, issue=3, pageStart=9, pageEnd=18, url=null, language=null, rfNumber=19, rfOrder=37, authorNames=QIN M, CHENG G X, LI Q, journalName=Pressure Vessel Technology, refType=null, unstructuredReference=QIN M,CHENG G X,LI Q,et al.Study of influence factors on quality of 2.25Cr-1Mo-0.25V steel for welded joint of hydrogenation reactor[J].Pressure Vessel Technology,2022,39(3):9-18., articleTitle=Study of influence factors on quality of 2.25Cr-1Mo-0.25V steel for welded joint of hydrogenation reactor, refAbstract=null)], funds=null, companyList=[AuthorCompany(id=1327335887752508342, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, xref=1, ext=[AuthorCompanyExt(id=1327335887760896951, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China), AuthorCompanyExt(id=1327335887769285560, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1二重(德阳)重型装备有限公司,四川 德阳 618000)]), AuthorCompany(id=1327335887836394425, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, xref=2, ext=[AuthorCompanyExt(id=1327335887848977338, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887836394425, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=2Sichuan Xiye New Material Co.,Ltd.,Chengdu 610000,China), AuthorCompanyExt(id=1327335887853171643, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887836394425, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=2四川西冶新材料股份有限公司,成都 610000)])], figs=[ArticleFig(id=1327335891443495907, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Fig.1, caption=Macroscopic morphology of SMAW, figureFileSmall=4iI+eMagd+rzpPCJIDEJ0g==, figureFileBig=U7kfPwSk2a+gUqapxSSHXg==, tableContent=null), ArticleFig(id=1327335891510604772, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=图1, caption=焊条电弧焊焊缝宏观形貌, figureFileSmall=4iI+eMagd+rzpPCJIDEJ0g==, figureFileBig=U7kfPwSk2a+gUqapxSSHXg==, tableContent=null), ArticleFig(id=1327335891695154149, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Fig.2, caption=Macroscopic morphology of narrow‑gap SAW, figureFileSmall=E/fx5AptNcijopc/8mThOw==, figureFileBig=ce1adEN6NS4La3SgA/S4aA==, tableContent=null), ArticleFig(id=1327335891762263014, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=图2, caption=窄间隙埋弧焊焊缝宏观形貌, figureFileSmall=E/fx5AptNcijopc/8mThOw==, figureFileBig=ce1adEN6NS4La3SgA/S4aA==, tableContent=null), ArticleFig(id=1327335891846149095, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Fig.3, caption=30 mm thick plate tensile specimen, figureFileSmall=4MdqStl1cARZFgb4cSCr7w==, figureFileBig=qojsQ93Gn9ghZuoDc7I3fQ==, tableContent=null), ArticleFig(id=1327335891946812392, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=图3, caption=30 mm厚板拉伸试样, figureFileSmall=4MdqStl1cARZFgb4cSCr7w==, figureFileBig=qojsQ93Gn9ghZuoDc7I3fQ==, tableContent=null), ArticleFig(id=1327335892018115561, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Fig.4, caption=Room‑temperature tensile test results of SMAW, figureFileSmall=K4ibS4uyUAr8fDyAzPUNfw==, figureFileBig=HA/XL4N2eovpgwyZtKn9qg==, tableContent=null), ArticleFig(id=1327335892093613034, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=图4, caption=焊条电弧焊室温拉伸试验结果, figureFileSmall=K4ibS4uyUAr8fDyAzPUNfw==, figureFileBig=HA/XL4N2eovpgwyZtKn9qg==, tableContent=null), ArticleFig(id=1327335892173304811, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Fig.5, caption=Room‑temperature tensile test results of single‑wire SAW, figureFileSmall=rFYT3SEmikBf3TI2/0oxOw==, figureFileBig=ThZs7OgZAGMSeDE55bioiw==, tableContent=null), ArticleFig(id=1327335892252996588, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=图5, caption=单丝埋弧焊室温拉伸试验结果, figureFileSmall=rFYT3SEmikBf3TI2/0oxOw==, figureFileBig=ThZs7OgZAGMSeDE55bioiw==, tableContent=null), ArticleFig(id=1327335892307522541, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Fig.6, caption=Room‑temperature tensile test results of twin‑wire SAW, figureFileSmall=UaOG6s9Xl8DhZ4uD74wYlQ==, figureFileBig=DMIVuUAJ9+4ZRVgZq8eoVA==, tableContent=null), ArticleFig(id=1327335892370437102, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=图6, caption=双丝埋弧焊室温拉伸试验结果, figureFileSmall=UaOG6s9Xl8DhZ4uD74wYlQ==, figureFileBig=DMIVuUAJ9+4ZRVgZq8eoVA==, tableContent=null), ArticleFig(id=1327335892437545967, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Fig.7, caption=Fracture morphology of room‑temperature all‑weld‑metal tensile specimen, figureFileSmall=2ZImNsbjUqd/Mq6J72Y/gw==, figureFileBig=cSaTVPwS4BE8NFcgivtXHA==, tableContent=null), ArticleFig(id=1327335892496266224, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=图7, caption=室温全焊缝拉伸断裂试样, figureFileSmall=2ZImNsbjUqd/Mq6J72Y/gw==, figureFileBig=cSaTVPwS4BE8NFcgivtXHA==, tableContent=null), ArticleFig(id=1327335892575958001, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Fig.8, caption=Fracture morphology of high‑temperature tensile specimen, figureFileSmall=LktaVrt+QjFaamlky9vuPQ==, figureFileBig=6hyRIQOCe7LeZC9AXt7l0w==, tableContent=null), ArticleFig(id=1327335892655649778, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=图8, caption=高温拉伸试样断裂形貌, figureFileSmall=LktaVrt+QjFaamlky9vuPQ==, figureFileBig=6hyRIQOCe7LeZC9AXt7l0w==, tableContent=null), ArticleFig(id=1327335892777284595, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Fig.9, caption=Bending test specimen, figureFileSmall=gKzFX/u4V0ksRqIs5i8pVA==, figureFileBig=QOa/CYw6rAbdNT/wtdc9Vg==, tableContent=null), ArticleFig(id=1327335892852782068, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=图9, caption=弯曲试验试样, figureFileSmall=gKzFX/u4V0ksRqIs5i8pVA==, figureFileBig=QOa/CYw6rAbdNT/wtdc9Vg==, tableContent=null), ArticleFig(id=1327335892911502325, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Fig.10, caption=Step cooling process, figureFileSmall=SLYbyCUbVuuleEhzNSv7mQ==, figureFileBig=FrnljMNIQ+AFEo/1j2NP5w==, tableContent=null), ArticleFig(id=1327335892970222582, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=图10, caption=阶梯冷却工艺, figureFileSmall=SLYbyCUbVuuleEhzNSv7mQ==, figureFileBig=FrnljMNIQ+AFEo/1j2NP5w==, tableContent=null), ArticleFig(id=1327335893049914359, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Fig.11, caption=Relationship between impact absorbed energy and test temperature, figureFileSmall=PV4NwSM0br32XCuKoNBdAA==, figureFileBig=JQCB3o2L+Ol0OuHPY7KcZg==, tableContent=null), ArticleFig(id=1327335893125411832, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=图11, caption=冲击吸收能量与试验温度的关系, figureFileSmall=PV4NwSM0br32XCuKoNBdAA==, figureFileBig=JQCB3o2L+Ol0OuHPY7KcZg==, tableContent=null), ArticleFig(id=1327335893188326393, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Tab.1, caption=

Weld parameter

, figureFileSmall=null, figureFileBig=null, tableContent=
焊接方法电源极性预热温度/℃层间温度/℃电流/A电压/V焊接速度/(cm·min-1)最大热输入量/(kJ·cm-1)焊接位置
SAW(单丝)AC≥180≤250520~55031~3336~4230.25平焊
SAW(双丝)前丝DC+后丝AC≥180≤250480~52028~31(前丝)
30~33(后丝)
65~7014.80(前丝)
15.80(后丝)
平焊
SMAWDC≥180≤250160~18523~2612~1824.05平焊
), ArticleFig(id=1327335894874436602, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=表1, caption=

焊接参数

, figureFileSmall=null, figureFileBig=null, tableContent=
焊接方法电源极性预热温度/℃层间温度/℃电流/A电压/V焊接速度/(cm·min-1)最大热输入量/(kJ·cm-1)焊接位置
SAW(单丝)AC≥180≤250520~55031~3336~4230.25平焊
SAW(双丝)前丝DC+后丝AC≥180≤250480~52028~31(前丝)
30~33(后丝)
65~7014.80(前丝)
15.80(后丝)
平焊
SMAWDC≥180≤250160~18523~2612~1824.05平焊
), ArticleFig(id=1327335894945739771, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Tab.2, caption=

Chemical composition of weld metal

, figureFileSmall=null, figureFileBig=null, tableContent=
元素标准值取样位置单丝埋弧焊实测值双丝埋弧焊实测值焊条电弧焊实测值
C0.050~0.150T/20.080 00.090 00.070 0
T/40.080 00.070 00.070 0
Si0.050~0.350(SAW)
0.200~0.350(SMAW)
T/20.140 00.100 00.260 0
T/40.130 00.130 00.260 0
Mn0.500~1.300T/21.120 01.050 00.900 0
T/41.100 01.150 00.910 0
P≤0.010T/20.005 00.004 00.004 0
T/40.005 00.004 00.003 0
S≤0.010T/20.002 00.002 00.003 0
T/40.002 00.002 00.004 0
Cr2.000~2.600T/22.490 02.440 02.450 0
T/42.470 02.430 02.470 0
Mo0.900~1.200T/21.000 01.000 00.970 0
T/41.000 00.980 00.970 0
V0.200~0.400T/20.340 00.330 00.330 0
T/40.340 00.340 00.330 0
Ni≤0.250T/20.020 00.040 00.020 0
T/40.020 00.030 00.020 0
Cu≤0.200T/20.110 00.110 00.090 0
T/40.110 00.110 00.090 0
Nb0.010~0.040T/20.020 00.020 00.020 0
T/40.020 00.020 00.020 0
Ti≤0.030T/20.001 00.001 00.005 0
T/40.001 00.001 00.005 0
Sb≤0.003T/20.001 00.001 00.002 0
T/40.001 00.001 00.001 0
Sn≤0.010T/20.002 00.001 00.001 0
T/40.002 00.001 00.001 0
As≤0.012T/20.005 00.005 00.006 0
T/40.005 00.006 00.005 0
B≤0.002T/20.000 20.000 20.002 0
T/40.000 20.000 20.001 0
), ArticleFig(id=1327335895025431548, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=表2, caption=

焊缝金属化学成分

, figureFileSmall=null, figureFileBig=null, tableContent=
元素标准值取样位置单丝埋弧焊实测值双丝埋弧焊实测值焊条电弧焊实测值
C0.050~0.150T/20.080 00.090 00.070 0
T/40.080 00.070 00.070 0
Si0.050~0.350(SAW)
0.200~0.350(SMAW)
T/20.140 00.100 00.260 0
T/40.130 00.130 00.260 0
Mn0.500~1.300T/21.120 01.050 00.900 0
T/41.100 01.150 00.910 0
P≤0.010T/20.005 00.004 00.004 0
T/40.005 00.004 00.003 0
S≤0.010T/20.002 00.002 00.003 0
T/40.002 00.002 00.004 0
Cr2.000~2.600T/22.490 02.440 02.450 0
T/42.470 02.430 02.470 0
Mo0.900~1.200T/21.000 01.000 00.970 0
T/41.000 00.980 00.970 0
V0.200~0.400T/20.340 00.330 00.330 0
T/40.340 00.340 00.330 0
Ni≤0.250T/20.020 00.040 00.020 0
T/40.020 00.030 00.020 0
Cu≤0.200T/20.110 00.110 00.090 0
T/40.110 00.110 00.090 0
Nb0.010~0.040T/20.020 00.020 00.020 0
T/40.020 00.020 00.020 0
Ti≤0.030T/20.001 00.001 00.005 0
T/40.001 00.001 00.005 0
Sb≤0.003T/20.001 00.001 00.002 0
T/40.001 00.001 00.001 0
Sn≤0.010T/20.002 00.001 00.001 0
T/40.002 00.001 00.001 0
As≤0.012T/20.005 00.005 00.006 0
T/40.005 00.006 00.005 0
B≤0.002T/20.000 20.000 20.002 0
T/40.000 20.000 20.001 0
), ArticleFig(id=1327335895138677757, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Tab.3, caption=

Post‑weld heat treatment parameters

, figureFileSmall=null, figureFileBig=null, tableContent=
条件参数
Max.PWHT(705±14) ℃×34-0+2 h
Min.PWHT(705±14) ℃×8-2+0 h
), ArticleFig(id=1327335895511970814, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=表3, caption=

焊后热处理参数

, figureFileSmall=null, figureFileBig=null, tableContent=
条件参数
Max.PWHT(705±14) ℃×34-0+2 h
Min.PWHT(705±14) ℃×8-2+0 h
), ArticleFig(id=1327335895574885375, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Tab.4, caption=

All‑weld‑metal tensile test results of SMAW

, figureFileSmall=null, figureFileBig=null, tableContent=
项目取样位置抗拉强度Rm/MPa屈服强度Rp0.2/MPa延伸率A/%断面收缩率Z/%
室温拉伸Min.PWHTT/266755920.073
距离上表面1.6 mm68057618.571
距离下表面1.6 mm67556820.070
室温拉伸Max.PWHTT/261749721.573
距离上表面1.6 mm60247824.575
距离下表面1.6 mm62049923.574
), ArticleFig(id=1327335895629411328, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=表4, caption=

焊条电弧焊全焊缝拉伸试验结果

, figureFileSmall=null, figureFileBig=null, tableContent=
项目取样位置抗拉强度Rm/MPa屈服强度Rp0.2/MPa延伸率A/%断面收缩率Z/%
室温拉伸Min.PWHTT/266755920.073
距离上表面1.6 mm68057618.571
距离下表面1.6 mm67556820.070
室温拉伸Max.PWHTT/261749721.573
距离上表面1.6 mm60247824.575
距离下表面1.6 mm62049923.574
), ArticleFig(id=1327335895696519168, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Tab.5, caption=

All‑weld‑metal tensile test results of single‑wire SAW

, figureFileSmall=null, figureFileBig=null, tableContent=
项目取样位置抗拉强度Rm/MPa屈服强度Rp0.2/MPa延伸率A/%断面收缩率Z/%
室温拉伸Min.PWHTT/265954822.571
距离上表面1.6 mm65454522.572
距离下表面1.6 mm66155222.572
室温拉伸Max.PWHTT/260548725.574
距离上表面1.6 mm60848926.574
距离下表面1.6m m61949825.074
), ArticleFig(id=1327335895763628033, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=表5, caption=

单丝埋弧焊全焊缝拉伸试验结果

, figureFileSmall=null, figureFileBig=null, tableContent=
项目取样位置抗拉强度Rm/MPa屈服强度Rp0.2/MPa延伸率A/%断面收缩率Z/%
室温拉伸Min.PWHTT/265954822.571
距离上表面1.6 mm65454522.572
距离下表面1.6 mm66155222.572
室温拉伸Max.PWHTT/260548725.574
距离上表面1.6 mm60848926.574
距离下表面1.6m m61949825.074
), ArticleFig(id=1327335895834931202, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Tab.6, caption=

All‑weld‑metal tensile test results of twin‑wire SAW

, figureFileSmall=null, figureFileBig=null, tableContent=
项目取样位置抗拉强度Rm/MPa屈服强度Rp0.2/MPa延伸率A/%断面收缩率Z/%
室温拉伸Min.PWHTT/268257821.072
距离上表面1.6 mm65955222.074
距离下表面1.6 mm65654922.573
室温拉伸Max.PWHTT/261950025.073
距离上表面1.6 mm62050224.072
距离下表面1.6 mm61749823.573
), ArticleFig(id=1327335895902040067, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=表6, caption=

双丝埋弧焊全焊缝拉伸试验结果

, figureFileSmall=null, figureFileBig=null, tableContent=
项目取样位置抗拉强度Rm/MPa屈服强度Rp0.2/MPa延伸率A/%断面收缩率Z/%
室温拉伸Min.PWHTT/268257821.072
距离上表面1.6 mm65955222.074
距离下表面1.6 mm65654922.573
室温拉伸Max.PWHTT/261950025.073
距离上表面1.6 mm62050224.072
距离下表面1.6 mm61749823.573
), ArticleFig(id=1327335895981731844, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Tab.7, caption=

High‑temperature tensile test results of SMAW joint

, figureFileSmall=null, figureFileBig=null, tableContent=
项目取样位置抗拉强度Rm/MPa屈服强度Rp0.2/MPa延伸率A/%断面收缩率Z/%
454 ℃高温拉伸Min.PWHTT/249742813.578
距离上表面1.6 mm49742512.577
距离下表面1.6 mm49042014.579
454 ℃高温拉伸Max.PWHTT/247939917.071
距离上表面1.6 mm47639616.577
距离下表面1.6 mm46438416.570
), ArticleFig(id=1327335896044646405, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=表7, caption=

焊条电弧焊焊接接头高温拉伸试验结果

, figureFileSmall=null, figureFileBig=null, tableContent=
项目取样位置抗拉强度Rm/MPa屈服强度Rp0.2/MPa延伸率A/%断面收缩率Z/%
454 ℃高温拉伸Min.PWHTT/249742813.578
距离上表面1.6 mm49742512.577
距离下表面1.6 mm49042014.579
454 ℃高温拉伸Max.PWHTT/247939917.071
距离上表面1.6 mm47639616.577
距离下表面1.6 mm46438416.570
), ArticleFig(id=1327335896111755270, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Tab.8, caption=

High‑temperature tensile test results of single‑wire SAW joint

, figureFileSmall=null, figureFileBig=null, tableContent=
项目取样位置抗拉强度Rm/MPa屈服强度Rp0.2/MPa延伸率A/%断面收缩率Z/%
454 ℃高温拉伸Min.PWHTT/247540615.079
距离上表面1.6 mm49042015.577
距离下表面1.6 mm48041314.577
454 ℃高温拉伸Max.PWHTT/246538617.072
距离上表面1.6 mm46438816.577
距离下表面1.6 mm46938416.577
), ArticleFig(id=1327335896199835655, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=表8, caption=

单丝埋弧焊焊接接头高温拉伸试验结果

, figureFileSmall=null, figureFileBig=null, tableContent=
项目取样位置抗拉强度Rm/MPa屈服强度Rp0.2/MPa延伸率A/%断面收缩率Z/%
454 ℃高温拉伸Min.PWHTT/247540615.079
距离上表面1.6 mm49042015.577
距离下表面1.6 mm48041314.577
454 ℃高温拉伸Max.PWHTT/246538617.072
距离上表面1.6 mm46438816.577
距离下表面1.6 mm46938416.577
), ArticleFig(id=1327335896271138824, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Tab.9, caption=

High‑temperature tensile test results of twin‑wire SAW joint

, figureFileSmall=null, figureFileBig=null, tableContent=
项目取样位置抗拉强度Rm/MPa屈服强度Rp0.2/MPa延伸率A/%断面收缩率Z/%
454 ℃高温拉伸Min.PWHTT/249341315.577
距离上表面1.6 mm48240915.577
距离下表面1.6 mm49441315.073
454 ℃高温拉伸Max.PWHTT/248139716.078
距离上表面1.6 mm46937816.575
距离下表面1.6 mm46437117.076
), ArticleFig(id=1327335896338247689, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=表9, caption=

双丝埋弧焊焊接接头高温拉伸试验结果

, figureFileSmall=null, figureFileBig=null, tableContent=
项目取样位置抗拉强度Rm/MPa屈服强度Rp0.2/MPa延伸率A/%断面收缩率Z/%
454 ℃高温拉伸Min.PWHTT/249341315.577
距离上表面1.6 mm48240915.577
距离下表面1.6 mm49441315.073
454 ℃高温拉伸Max.PWHTT/248139716.078
距离上表面1.6 mm46937816.575
距离下表面1.6 mm46437117.076
), ArticleFig(id=1327335896413745162, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Tab.10, caption=

All‑weld‑metal high‑temperature tensile test results of SMAW

, figureFileSmall=null, figureFileBig=null, tableContent=
项目取样位置抗拉强度Rm/MPa屈服强度Rp0.2/MPa延伸率A/%断面收缩率Z/%
454 ℃高温拉伸Min.PWHTT/252546115.569
距离上表面1.6 mm52045516.068
距离下表面1.6 mm50944615.069
454 ℃高温拉伸Max.PWHTT/247140017.071
距离上表面1.6 mm47740618.071
距离下表面1.6 mm47640318.070
), ArticleFig(id=1327335896535379979, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=表10, caption=

焊条电弧焊全焊缝高温拉伸试验结果

, figureFileSmall=null, figureFileBig=null, tableContent=
项目取样位置抗拉强度Rm/MPa屈服强度Rp0.2/MPa延伸率A/%断面收缩率Z/%
454 ℃高温拉伸Min.PWHTT/252546115.569
距离上表面1.6 mm52045516.068
距离下表面1.6 mm50944615.069
454 ℃高温拉伸Max.PWHTT/247140017.071
距离上表面1.6 mm47740618.071
距离下表面1.6 mm47640318.070
), ArticleFig(id=1327335896615071756, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Tab.11, caption=

All‑weld‑metal high‑temperature tensile test results of single‑wire SAW

, figureFileSmall=null, figureFileBig=null, tableContent=
项目取样位置抗拉强度Rm/MPa屈服强度Rp0.2/MPa延伸率A/%断面收缩率Z/%
454 ℃高温拉伸Min.PWHTT/250544715.570
距离上表面1.6 mm51847518.573
距离下表面1.6 mm50444515.572
454 ℃高温拉伸Max.PWHTT/247339319.072
距离上表面1.6 mm46439919.575
距离下表面1.6 mm46340518.572
), ArticleFig(id=1327335896711540749, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=表11, caption=

单丝埋弧焊全焊缝高温拉伸试验结果

, figureFileSmall=null, figureFileBig=null, tableContent=
项目取样位置抗拉强度Rm/MPa屈服强度Rp0.2/MPa延伸率A/%断面收缩率Z/%
454 ℃高温拉伸Min.PWHTT/250544715.570
距离上表面1.6 mm51847518.573
距离下表面1.6 mm50444515.572
454 ℃高温拉伸Max.PWHTT/247339319.072
距离上表面1.6 mm46439919.575
距离下表面1.6 mm46340518.572
), ArticleFig(id=1327335896778649614, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Tab.12, caption=

All‑weld‑metal high‑temperature tensile test results of twin‑wire SAW

, figureFileSmall=null, figureFileBig=null, tableContent=
项目取样位置抗拉强度Rm/MPa屈服强度Rp0.2/MPa延伸率A/%断面收缩率Z/%
454 ℃高温拉伸Min.PWHTT/252145615.568
距离上表面1.6 mm52946515.568
距离下表面1.6 mm53146615.567
454 ℃高温拉伸Max.PWHTT/247640415.562
距离上表面1.6 mm47740118.072
距离下表面1.6 mm48140818.071
), ArticleFig(id=1327335896833175567, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=表12, caption=

双丝埋弧焊全焊缝高温拉伸试验结果

, figureFileSmall=null, figureFileBig=null, tableContent=
项目取样位置抗拉强度Rm/MPa屈服强度Rp0.2/MPa延伸率A/%断面收缩率Z/%
454 ℃高温拉伸Min.PWHTT/252145615.568
距离上表面1.6 mm52946515.568
距离下表面1.6 mm53146615.567
454 ℃高温拉伸Max.PWHTT/247640415.562
距离上表面1.6 mm47740118.072
距离下表面1.6 mm48140818.071
), ArticleFig(id=1327335896896090128, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Tab.13, caption=

Impact test results at -30 ℃

, figureFileSmall=null, figureFileBig=null, tableContent=
焊接方法冲击试样V型缺口位置冲击吸收能量KV2/J侧向膨胀值/mm纤维状断口百分比/%
单丝SAW焊缝中心T/2139,134,1541.77,1.78,1.8765,70,75
热影响区T/2200,206,2302.19,2.06,2.1495,100,100
母材T/2141,264,2381.73,2.15,2.1350,100,100
双丝SAW焊缝中心T/2165,112,1222.07,1.65,1.7175,65,65
热影响区T/2253,267,2072.30,2.50,2.34100,100,80
母材T/2274,280,2942.34,2.43,2.40100,100,100
SMAW焊缝中心T/2148,159,1571.80,2.02,1.9470,75,75
热影响区T/2189,224,1912.16,2.27,2.03100,80,100
母材T/2258,256,2612.16,2.05,2.00100,100,100
), ArticleFig(id=1327335896963198993, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=表13, caption=

-30 ℃冲击试验结果

, figureFileSmall=null, figureFileBig=null, tableContent=
焊接方法冲击试样V型缺口位置冲击吸收能量KV2/J侧向膨胀值/mm纤维状断口百分比/%
单丝SAW焊缝中心T/2139,134,1541.77,1.78,1.8765,70,75
热影响区T/2200,206,2302.19,2.06,2.1495,100,100
母材T/2141,264,2381.73,2.15,2.1350,100,100
双丝SAW焊缝中心T/2165,112,1222.07,1.65,1.7175,65,65
热影响区T/2253,267,2072.30,2.50,2.34100,100,80
母材T/2274,280,2942.34,2.43,2.40100,100,100
SMAW焊缝中心T/2148,159,1571.80,2.02,1.9470,75,75
热影响区T/2189,224,1912.16,2.27,2.03100,80,100
母材T/2258,256,2612.16,2.05,2.00100,100,100
), ArticleFig(id=1327335897017724946, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Tab.14, caption=

Temper embrittlement susceptibility test results

, figureFileSmall=null, figureFileBig=null, tableContent=
焊接方法焊缝区域vTr54+3ΔvTr54/℃热影响区vTr54+3ΔvTr54/℃
单丝SAW-49.6-64.6
双丝SAW-37.6-48.6
SMAW-16.3-102.8
), ArticleFig(id=1327335897084833811, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=表14, caption=

回火脆化倾向试验结果

, figureFileSmall=null, figureFileBig=null, tableContent=
焊接方法焊缝区域vTr54+3ΔvTr54/℃热影响区vTr54+3ΔvTr54/℃
单丝SAW-49.6-64.6
双丝SAW-37.6-48.6
SMAW-16.3-102.8
), ArticleFig(id=1327335897143554068, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Tab.15, caption=

High‑temperature creep rupture strength test results

, figureFileSmall=null, figureFileBig=null, tableContent=
焊接方法试样状态试样位置试验温度/℃试验应力/MPa试验时间/h断裂状态
SAW单丝Max.PWHTT/2纵向全焊缝5402101 101.0断面光滑
SAW单丝Max.PWHTT/2横向接头5402101 258.7断面光滑
SAW双丝Max.PWHTT/2纵向全焊缝5402101 193断面光滑
SAW双丝Max.PWHTT/2横向接头5402101 177断面光滑
), ArticleFig(id=1327335897202274325, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=表15, caption=

高温持久强度试验结果

, figureFileSmall=null, figureFileBig=null, tableContent=
焊接方法试样状态试样位置试验温度/℃试验应力/MPa试验时间/h断裂状态
SAW单丝Max.PWHTT/2纵向全焊缝5402101 101.0断面光滑
SAW单丝Max.PWHTT/2横向接头5402101 258.7断面光滑
SAW双丝Max.PWHTT/2纵向全焊缝5402101 193断面光滑
SAW双丝Max.PWHTT/2横向接头5402101 177断面光滑
), ArticleFig(id=1327335897294549014, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Tab.16, caption=

Kf values

, figureFileSmall=null, figureFileBig=null, tableContent=
项目PbBiSbKf
焊丝9.0×10-71.5×10-87.98×10-61.15×10-6
熔敷金属16.6×10-71.0×10-78.74×10-61.02×10-6
熔敷金属26.8×10-71.2×10-76.84×10-61.01×10-6
), ArticleFig(id=1327335897365852183, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=表16, caption=

Kf系数

, figureFileSmall=null, figureFileBig=null, tableContent=
项目PbBiSbKf
焊丝9.0×10-71.5×10-87.98×10-61.15×10-6
熔敷金属16.6×10-71.0×10-78.74×10-61.02×10-6
熔敷金属26.8×10-71.2×10-76.84×10-61.01×10-6
), ArticleFig(id=1327335897432961048, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=EN, label=Tab.17, caption=

Gleeble test results

, figureFileSmall=null, figureFileBig=null, tableContent=
测试温度T/℃初始直径d0/mm断口直径d1/mm断面收缩率/%最大拉力/kgf变形速率/s-1
6508.006.5433.173 311.45×10-4
6507.996.5632.593 2955×10-4
6508.006.3636.803 3325×10-4
), ArticleFig(id=1327335897487487001, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, language=CN, label=表17, caption=

Gleeble试验结果

, figureFileSmall=null, figureFileBig=null, tableContent=
测试温度T/℃初始直径d0/mm断口直径d1/mm断面收缩率/%最大拉力/kgf变形速率/s-1
6508.006.5433.173 311.45×10-4
6507.996.5632.593 2955×10-4
6508.006.3636.803 3325×10-4
)], attaches=null, journal=Journal(id=1319354845020389520, delFlag=0, nameCn=压力容器, nameEn=Pressure Vessel Technology, nameHistory1=null, nameHistory2=null, issn=1001-4837, eissn=null, cn=34-1058/TH, coden=null, periodic=0, language=CN, oaType=null, ccby=null, superviseOffice=null, ownerOffice=null, pubOffice=null, editorOffice=null, officeType=null, aims=null, clcCode=null, officeProv=null, officeCity=null, officeAddr=null, officeZip=null, officeEmail=null, officePhone=null, editDirector=null, officeDirector=null, officeDirectorPhone=null, officeStaffNum=null, officeEmpNum=null, coverPicUrl=jxjNdnQvHSQ8b9q0zS7Bgw==, journalPrice=null, startedYear=null, abbrevIsoEn=Pressure Vessel Technology, journalRemark=null, publicationField=null, createdTime=1792488307482, updatedTime=1792488496537, createdBy=18614031015, updatedBy=13701087609, firstLetterCn=Y, firstLetterEn=Y, subjectCode=Engineering, subjectName=null, subjectCodeEn=Engineering, subjectNameEn=null, picCn=jxjNdnQvHSQ8b9q0zS7Bgw==, picEn=4fVBwqRFt4uCO8g42aXObg==, jcr=null, cjcr=null, exts=[JournalExt(id=1319355638048740090, language=CN, name=压力容器, nameHistory1=null, nameHistory2=null, managedBy=, sponsoredBy=, publishedBy=, editorOffice=, officeProv=null, officeCity=null, officeAddr=, officeZip=, editDirector=, officeDirector=null, officePhone=null, coverPicUrl=null, journalRemark=, submitArticleUrl=null, websiteUrl=, createdTime=1792488496553, updatedTime=1792488496553, createdBy=13701087609, updatedBy=13701087609, submissionGuidelinesUrl=, submissionAuthorUrl=https://ylrq.portal.founderss.cn, submissionEditorUrl=https://journal.ids.fzyun.cn, submissionReviewUrl=https://ylrq.portal.founderss.cn, submissionCeEditorUrl=, submissionAeEditorUrl=, option={"copyright":""}), JournalExt(id=1319355638103266043, language=EN, name=Pressure Vessel Technology, nameHistory1=null, nameHistory2=null, managedBy=, sponsoredBy=, publishedBy=, editorOffice=, officeProv=null, officeCity=null, officeAddr=, officeZip=, editDirector=, officeDirector=null, officePhone=null, coverPicUrl=null, journalRemark=, submitArticleUrl=null, websiteUrl=, createdTime=1792488496566, updatedTime=1792488496566, createdBy=13701087609, updatedBy=13701087609, submissionGuidelinesUrl=, submissionAuthorUrl=https://ylrq.portal.founderss.cn, submissionEditorUrl=https://journal.ids.fzyun.cn, submissionReviewUrl=https://ylrq.portal.founderss.cn, submissionCeEditorUrl=, submissionAeEditorUrl=, option={"copyright":""})], databaseList=null, tenantJournalId=1319355204128309394, websiteList=[Website(id=1319376331645764504, webName=null, webTitle=null, webDomain=null, webCopyrigh=null, webIpcNo=null, seoTitle=null, seoKeywords=null, seoDescription=null, tenantJournalId=null, journalId=1319355204128309394, journalNameCn=null, journalNameEn=null, grayFlag=null, tenantId=1146029695717560320, platformId=null, journalGroupId=null, journalGroupNameCn=null, journalGroupNameEn=null, type=1, domain=https://castjournals.cast.org.cn/joweb/ylrq/CN, language=CN, createTime=1792493430291, createBy=18614031015, updateTime=1792493471510, updateBy=18614031015, name=压力容器-中文, tplId=1146099689490845704, title=压力容器, delFlag=0, indexPage=/home, props=[WebsiteProps(id=1319376610952856568, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=articleTextType, value=kx, createTime=1792493496883, updateTime=1792493496883, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610923496437, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=banner, value=null, createTime=1792493496876, updateTime=1792493496876, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610969633787, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=grayFlag, value=0, createTime=1792493496887, updateTime=1792493496887, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610910913524, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=logo, value=https://castjournals.cast.org.cn/joweb/ylrq/CN/file/pic?fileId=jTQ3ULyAlxRu0s8fI4nfng==, createTime=1792493496873, updateTime=1792493496873, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610986411005, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=minRunFlag, value=0, createTime=1792493496891, updateTime=1792493496891, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610944467959, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=picServerUrl, value=https://castjournals.cast.org.cn/joweb/ylrq/CN/file/pic, createTime=1792493496881, updateTime=1792493496881, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610978022396, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=silenceFlag, value=0, createTime=1792493496889, updateTime=1792493496889, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610936079350, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=staticResourcePath, value=https://castjournals.cast.org.cn/joweb/cast_kjdb_cn_619/, createTime=1792493496879, updateTime=1792493496879, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610957050873, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=themeColor, value=null, createTime=1792493496884, updateTime=1792493496884, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610965439482, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=themeStyle, value=null, createTime=1792493496886, updateTime=1792493496886, creator=18614031015, updator=18614031015)]), Website(id=1319376331893228450, webName=null, webTitle=null, webDomain=null, webCopyrigh=null, webIpcNo=null, seoTitle=null, seoKeywords=null, seoDescription=null, tenantJournalId=null, journalId=1319355204128309394, journalNameCn=null, journalNameEn=null, grayFlag=null, tenantId=1146029695717560320, platformId=null, journalGroupId=null, journalGroupNameCn=null, journalGroupNameEn=null, type=1, domain=https://castjournals.cast.org.cn/joweb/ylrq/EN, language=EN, createTime=1792493430350, createBy=18614031015, updateTime=1792493467616, updateBy=18614031015, name=压力容器-英文, tplId=1146101810881728533, title=Pressure Vessel Technology, delFlag=0, indexPage=/home, props=[WebsiteProps(id=1319376586462315499, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=articleTextType, value=kx, createTime=1792493491044, updateTime=1792493491044, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586432955368, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=banner, value=null, createTime=1792493491037, updateTime=1792493491037, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586500064238, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=grayFlag, value=0, createTime=1792493491053, updateTime=1792493491053, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586420372455, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=logo, value=https://castjournals.cast.org.cn/joweb/ylrq/EN/file/pic?fileId=jTQ3ULyAlxRu0s8fI4nfng==, createTime=1792493491034, updateTime=1792493491034, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586521035760, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=minRunFlag, value=0, createTime=1792493491058, updateTime=1792493491058, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586453926890, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=picServerUrl, value=https://castjournals.cast.org.cn/joweb/ylrq/EN/file/pic, createTime=1792493491042, updateTime=1792493491042, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586512647151, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=silenceFlag, value=0, createTime=1792493491056, updateTime=1792493491056, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586441343977, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=staticResourcePath, value=https://castjournals.cast.org.cn/joweb/cast_kjdb_en_623/, createTime=1792493491039, updateTime=1792493491039, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586474898412, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=themeColor, value=null, createTime=1792493491047, updateTime=1792493491047, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586487481325, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=themeStyle, value=null, createTime=1792493491050, updateTime=1792493491050, creator=18614031015, updator=18614031015)])], journalTitle=压力容器, weixinUrl=null, journalUrl=https://www.pvtjournal.com/, iacademicId=null, status=1, seqNo=null, journalTitleEn=Pressure Vessel Technology, journalPhotoCn=jxjNdnQvHSQ8b9q0zS7Bgw==, journalPhotoEn=4fVBwqRFt4uCO8g42aXObg==, journalFirstLetter=Y, journalRecommend=null, journalNew=null, journalCollection=null, jcrJf=null, cjcrJf=null, jcrJfStr=null, cjcrJfStr=null, submissionFirstDecision=null, sciSubjectClassification=null, casSubjectClassification=null, citeScore=null, totalCitationFrequency=null, icpCode=null, psCode=null, advertisingLicenseCode=null, copyrightInformation=null, country=null, option=, provinceCode=null, provinceName=null, collectFlag=false, interPubPlatform=, interPubPlatformUrl=null), detailUrlCn=https://castjournals.cast.org.cn/joweb/ylrq/CN/10.3969/j.issn.1001-4837.2025.11.002, detailUrlEn=https://castjournals.cast.org.cn/joweb/ylrq/EN/10.3969/j.issn.1001-4837.2025.11.002, pdfUrlCn=https://castjournals.cast.org.cn/joweb/ylrq/CN/PDF/10.3969/j.issn.1001-4837.2025.11.002, pdfUrlEn=https://castjournals.cast.org.cn/joweb/ylrq/EN/PDF/10.3969/j.issn.1001-4837.2025.11.002, aliStartDate=0, aliEndDate=0, collectionFlag=false, citedCount=null, citedUrl=null, previewStatus=0, delFlag=0, hasFullText=1, orderTime=1764432000000, fullTextJson=null, articleText=null, reference=null)
收藏切换
12Cr2Mo1V钢制加氢反应器主焊缝国产焊材工业化应用研究
吴成林 1 , 万敏 1 , 郭太平 1 , 王迎君 1 , 楚成刚 2 , 王雪骄 1
压力容器 | 试验研究 2025,42(11): 11-22
收起
收藏切换
压力容器 |试验研究 2025 , 42 (11) : 11 -22
12Cr2Mo1V钢制加氢反应器主焊缝国产焊材工业化应用研究
全屏
[Author(id=1327335887920280509, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, orderNo=0, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=908499928@qq.com, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335887995777983, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335887920280509, language=EN, stringName=Chenglin WU, firstName=Chenglin, middleName=null, lastName=WU, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335888075469760, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335887920280509, language=CN, stringName=吴成林, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1二重(德阳)重型装备有限公司,四川 德阳 618000, bio={"content":"

吴成林(1988),男,高级工程师,主要从事核电与压力容器焊接工艺技术工作,通信地址:618000四川省德阳市旌阳区珠江西路460号二重(德阳)重型装备有限公司核电石化公司核容所,E-mail:。

"}, bioImg=null, bioContent=

吴成林(1988),男,高级工程师,主要从事核电与压力容器焊接工艺技术工作,通信地址:618000四川省德阳市旌阳区珠江西路460号二重(德阳)重型装备有限公司核电石化公司核容所,E-mail:。

, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335887752508342, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, xref=1, ext=[AuthorCompanyExt(id=1327335887760896951, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China), AuthorCompanyExt(id=1327335887769285560, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1二重(德阳)重型装备有限公司,四川 德阳 618000)])]), Author(id=1327335888146772930, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, orderNo=1, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335888213881796, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335888146772930, language=EN, stringName=Min WAN, firstName=Min, middleName=null, lastName=WAN, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335888272602053, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335888146772930, language=CN, stringName=万敏, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1二重(德阳)重型装备有限公司,四川 德阳 618000, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335887752508342, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, xref=1, ext=[AuthorCompanyExt(id=1327335887760896951, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China), AuthorCompanyExt(id=1327335887769285560, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1二重(德阳)重型装备有限公司,四川 德阳 618000)])]), Author(id=1327335888348099527, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, orderNo=2, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335888440374217, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335888348099527, language=EN, stringName=Taiping GUO, firstName=Taiping, middleName=null, lastName=GUO, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335888503288778, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335888348099527, language=CN, stringName=郭太平, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1二重(德阳)重型装备有限公司,四川 德阳 618000, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335887752508342, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, xref=1, ext=[AuthorCompanyExt(id=1327335887760896951, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China), AuthorCompanyExt(id=1327335887769285560, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1二重(德阳)重型装备有限公司,四川 德阳 618000)])]), Author(id=1327335888562009036, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, orderNo=3, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335888637506510, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335888562009036, language=EN, stringName=Yingjun WANG, firstName=Yingjun, middleName=null, lastName=WANG, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335888704615375, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335888562009036, language=CN, stringName=王迎君, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1二重(德阳)重型装备有限公司,四川 德阳 618000, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335887752508342, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, xref=1, ext=[AuthorCompanyExt(id=1327335887760896951, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China), AuthorCompanyExt(id=1327335887769285560, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1二重(德阳)重型装备有限公司,四川 德阳 618000)])]), Author(id=1327335890403308497, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, orderNo=4, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335890483000275, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335890403308497, language=EN, stringName=Chenggang CHU, firstName=Chenggang, middleName=null, lastName=CHU, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=2, address=2Sichuan Xiye New Material Co.,Ltd.,Chengdu 610000,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335890550109140, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335890403308497, language=CN, stringName=楚成刚, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=2, address=2四川西冶新材料股份有限公司,成都 610000, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335887836394425, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, xref=2, ext=[AuthorCompanyExt(id=1327335887848977338, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887836394425, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=2Sichuan Xiye New Material Co.,Ltd.,Chengdu 610000,China), AuthorCompanyExt(id=1327335887853171643, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887836394425, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=2四川西冶新材料股份有限公司,成都 610000)])]), Author(id=1327335890604635094, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, orderNo=5, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335890680132568, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335890604635094, language=EN, stringName=Xuejiao WANG, firstName=Xuejiao, middleName=null, lastName=WANG, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335890751435737, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, authorId=1327335890604635094, language=CN, stringName=王雪骄, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1二重(德阳)重型装备有限公司,四川 德阳 618000, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335887752508342, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, xref=1, ext=[AuthorCompanyExt(id=1327335887760896951, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China), AuthorCompanyExt(id=1327335887769285560, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335883793085341, companyId=1327335887752508342, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1二重(德阳)重型装备有限公司,四川 德阳 618000)])])]
吴成林1 , 万敏1, 郭太平1, 王迎君1, 楚成刚2, 王雪骄1
作者信息
  • 1二重(德阳)重型装备有限公司,四川 德阳 618000
  • 2四川西冶新材料股份有限公司,成都 610000
作者简介:

吴成林(1988),男,高级工程师,主要从事核电与压力容器焊接工艺技术工作,通信地址:618000四川省德阳市旌阳区珠江西路460号二重(德阳)重型装备有限公司核电石化公司核容所,E-mail:。

Industrial application research of domestic welding materials for main weld seams of 12Cr2Mo1V steel hydrotreating reactors
Chenglin WU1 , Min WAN1, Taiping GUO1, Yingjun WANG1, Chenggang CHU2, Xuejiao WANG1
Affiliations
  • 1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China
  • 2Sichuan Xiye New Material Co.,Ltd.,Chengdu 610000,China
出版时间: 2025-11-30 doi: 10.3969/j.issn.1001-4837.2025.11.002
文章导航
收藏切换

针对12Cr2Mo1V钢加氢反应器主焊缝焊接材料长期依赖进口导致的采购周期长、成本高的问题,提出采用国产焊材替代并依据NB/T 47014—2023《承压设备焊接工艺评定》开展系统焊接试验的解决方案。结果表明,国产焊接接头的拉伸、冲击、弯曲、回火脆化倾向及高温蠕变等性能均满足设备制造要求,达到同类进口产品水平,部分数据更优。该焊材已成功应用于多台反应器主焊缝制造,实现了工业化应用。研究为推进该类高端焊接材料国产化、降低制造成本与缩短交付周期提供了实践依据与参考。

12Cr2Mo1V钢  /  加氢反应器  /  焊材国产化  /  工业化应用

To address the issues of long procurement cycles and high costs caused by long term reliance on imported welding materials for the main weld seams of 12Cr2Mo1V steel hydrotreating reactors,a solution is proposed that involves adopting domestic welding materials and conducting systematic welding tests in accordance with NB/T 47014—2023 Welding procedure qualification for pressure equipments.The results show that the properties of the domestic welded joints,including tensile strength,impact toughness,bending performance,temper embrittlement susceptibility,and high temperature creep resistance,all meet equipment manufacturing requirements,reaching the level of similar imported products,with some data being even better.These welding materials have been successfully applied to the manufacturing of main weld seams in multiple reactors,achieving industrial application.The study provides practical evidence and references for advancing the localization of such high end welding materials,reducing manufacturing costs,and shortening delivery cycles.

12Cr2Mo1V steel  /  hydrotreating reactor  /  localization of welding materials  /  industrial application
吴成林, 万敏, 郭太平, 王迎君, 楚成刚, 王雪骄. 12Cr2Mo1V钢制加氢反应器主焊缝国产焊材工业化应用研究. 压力容器, 2025 , 42 (11) : 11 -22 . DOI: 10.3969/j.issn.1001-4837.2025.11.002
Chenglin WU, Min WAN, Taiping GUO, Yingjun WANG, Chenggang CHU, Xuejiao WANG. Industrial application research of domestic welding materials for main weld seams of 12Cr2Mo1V steel hydrotreating reactors[J]. Pressure Vessel Technology, 2025 , 42 (11) : 11 -22 . DOI: 10.3969/j.issn.1001-4837.2025.11.002
12Cr2Mo1V钢制加氢反应器作为石化加氢装置的核心设备,其本体与堆焊层材料已实现国产化,性能符合设计及相关标准要求[1]。然而,主焊缝焊接材料仍长期依赖进口,存在采购周期长(常超过6个月)、成本高等突出问题。若能实现该类焊材的国产化替代,将大幅缩短采购周期、降低制造成本。
为此,文中基于NB/T 47014—2023《承压设备焊接工艺评定》等相关标准,采用国内某公司研发的12Cr2Mo1V钢配套焊材,系统开展工业化应用研究。重点对其焊接工艺性能(电弧稳定性、焊缝成形与脱渣性等)、化学成分匹配性、硬度分布、力学性能(抗拉强度、冲击韧性、弯曲)及长期服役条件下的回火脆化倾向[2]等关键指标进行了综合评价,并与同类进口产品性能进行对比。
该国产焊材的研发与应用,旨在为我国高端加氢反应器焊接材料的自主化提供实践支撑,以期为推动石化装备关键材料全面国产化、降低行业成本与提升供应链安全性提供参考。
目前,加氢反应器主焊缝主要采用焊条电弧焊和埋弧焊,其中埋弧焊应用占比约90%,并进一步分为单丝埋弧焊和双丝埋弧焊。双丝窄间隙埋弧自动焊接技术采用双焊丝同步施焊,具有焊接效率高、生产周期短的特点,已在国内外加氢反应器制造中得到广泛应用[3]。
依据12Cr2Mo1V钢制加氢反应器工程制造技术文件及相关标准(如NB/T 47014—2023)的要求,并结合当前压力容器向高温、高压、深冷、超大容积与超大壁厚方向发展的趋势,文中通过优化焊接参数,使焊缝各项性能指标满足技术规范,具体试验方案如下:
采用厚度为310 mm的12Cr2Mo1V(IV级)锻件作为焊接试件母材,选用手工焊条电弧焊(shielded metal arc welding,SMAW)、单丝及双丝窄间隙自动埋弧焊(submerged arc welding,SAW)进行对接焊接,共制备3组焊接试件。焊后对焊接接头进行无损检测:按NB/T 47013.4—2015《承压设备无损检测 第4部分:磁粉检测》执行100%磁粉检测(MT),要求检测等级Ⅰ级、质量等级Ⅰ级合格;按NB/T 47013.3—2023《承压设备无损检测 第3部分:超声检测》执行100%超声检测(UT),检测等级为Ⅰ级。
无损检测合格后,在焊态下进行化学成分分析。焊接试件经模拟12Cr2Mo1V钢制加氢反应器焊后热处理后,开展拉伸、低温冲击、弯曲、回火脆化倾向及硬度分布等性能试验,以评估国产主焊缝焊接材料是否满足设备制造要求。同时,通过焊接工艺性能、化学成分及理化性能检测等对比试验,将该国产焊材与同类进口焊材进行系统对比[4],检验其是否达到国外同类产品水平。
焊接工艺评定依据NB/T 47014—2023执行,评定合格后,将该国产焊材应用于大型加氢反应器主焊缝制造中,以实现批量化工业应用。3种焊接方法的详细工艺规范参数见表1。
采用国内某公司生产的埋弧焊丝(牌号XY-SCr2MoV)+焊剂(牌号XY-AF605)、焊条(牌号XY-ECr2MoV),分别通过单丝窄间隙埋弧焊、双丝窄间隙埋弧焊及焊条电弧焊3种方法开展焊接试验。焊接过程中,焊条电弧稳定、飞溅量小,焊缝成形均匀美观,尤其在复杂位置焊接时仍能保持良好的熔敷效果,显著减少了后续打磨修整的工作量;同时,其优异的脱渣性能可使焊渣轻松剥离,大幅提升连续作业效率,缩短因清渣导致的停工时间,焊条电弧焊焊缝宏观形貌见图1。
在埋弧焊丝方面,该焊材在单丝及双丝工艺中均表现出良好的适应性。单丝焊接时熔深适中、焊缝成型平滑;双丝焊接则通过合理分配热输入,在提升焊接速度的同时保障了成型质量。此外,该埋弧焊丝脱渣性能优异,焊后熔渣自动翘起剥离,有效避免了夹渣等常见缺陷,为自动化焊接提供了可靠保证。窄间隙埋弧焊焊缝的宏观形貌见图2。
焊缝的化学成分检测是控制与评价焊接质量的核心环节。通过对焊缝区域进行成分测定,可判断所选焊接材料与母材是否具有良好的相容性和匹配性,从而降低因合金元素偏离预期而导致强度不足或韧性下降的风险。
该分析还能准确测定硫、磷、氢等有害元素的含量,有助于预防焊接气孔、热裂纹等缺陷的形成,提高接头在服役中的可靠性与耐久性[5],为焊接参数的选取与优化、后续热处理制度的制定以及构件在役性能的预测提供了关键依据[6],从制造源头保障产品的整体质量与结构完整性。焊缝金属化学成分的分析结果如表2所示。
分别在焊缝厚度方向的T/2(中心区域)和T/4(过渡区域)位置取样检测,对3种焊接方法的焊缝金属进行化学成分分析,结果显示所有指标均符合ASME BPVC.Ⅷ.2—2023 Rules for Construction of Pressure Vessels-Division 2 Alternative Rules的要求。
X系数是量化焊缝中残余元素(P,Sb,Sn,As)致热裂纹倾向的经验模型,其计算方法如下:
X=(10P+5Sb+4Sn+As)×10-2
根据表1数据计算,3种焊接方法的X系数最大值为8×10-6,满足API RP 934-A—2019 Materials and Fabrication of 2¼Cr-1Mo-¼V,3Cr-1Mo,and 3Cr-1Mo-¼V Steel Heavy Wall Pressure Vessels for High‑temperature,High‑pressure Hydrogen Service中X系数不大于1.2×10-5的要求。
焊缝区域成分均匀性良好,未观察到明显的成分偏析,表明焊接热过程与冶金反应控制有效,微观组织稳定性较高。
焊接过程中剧烈的升降温循环会导致焊缝及热影响区产生较高的残余应力,容易引发开裂或应力腐蚀等缺陷[7]。为确保高压容器的使用安全,必须在焊后彻底消除残余应力、抑制氢脆倾向,并全面提升接头的韧性及组织稳定性。因此,对于12Cr2Mo1V,标准ASME BPVC.Ⅷ.2—2023明确规定需进行焊后热处理。该工艺通过合理的热处理制度(温度与时间)促使应力均匀释放,同时保持钢材原有性能不发生劣化[8],从而有效预防缺陷产生,保障设备长期运行的安全性与使用寿命。
为真实模拟实际产品制造与使用中所经历的热处理条件,3件焊接试板实际采用的焊后消应力热处理参数见表3。其中,Min.PWHT模拟制造过程中所有焊接完成后实施的最低程度焊后热处理(即最短保温时间与最低温度);Max.PWHT则模拟制造全过程可能经历的最严苛热处理条件,包括最终焊后热处理、一次可能的工厂返修焊后热处理,以及至少一次预留的后续使用中可能实施的额外焊后热处理。
所有焊接试板均切成两半,分别进行12Cr2Mo1V钢加氢反应器制造过程中的最小模拟焊后热处理(Min.PWHT)与最大模拟焊后热处理(Max.PWHT),并在相应热处理后进行性能测试。
通过室温拉伸试验测定焊接接头的极限强度。根据NB/T 47014—2023标准要求,当试件厚度大于30 mm时,可在其厚度方向均匀分层取样。因此,3件厚度为310 mm的焊接试件需在厚度方向均匀分层取样以开展拉伸试验。每件试样尺寸为30 mm×40 mm×370 mm,沿试板厚度方向分10层加工拉伸试样,试样方向垂直于焊缝,试样外观如图3所示。
12Cr2Mo1V锻件母材的抗拉强度要求范围为585~760 MPa。如图3所示,所有拉伸试样均断裂于母材;结合图4~图6的试验结果可知,焊接接头的抗拉强度不低于母材要求。
上述焊接接头的室温拉伸试验结果表明,整个焊接接头(含焊缝金属、熔合线、热影响区及两侧母材)的强度均满足标准要求,印证了焊材与母材的良好匹配性。为排除母材对强度的贡献,直接反映填充金属(焊材)与焊接工艺所形成的焊缝金属本身的强度与塑性,在试板T/2处及距上、下表面1.6 mm处分别加工了全焊缝拉伸试样。试样尺寸为⌀12.5 mm×110 mm,方向平行于焊缝,具体试验结果见表4~表6,试样断裂形貌如图7所示。
通过焊接接头高温拉伸测试,评价压力容器焊件在模拟高温工况下的力学性能与失效风险。该测试能有效揭示接头在高温下的薄弱区域(如焊缝、熔合线或热影响区),并分析焊缝金属、热影响区及母材在热载荷下的变形协调性,从而避免因局部塑性不足而导致早期失效[9]。通过该试验,可验证所选焊材、焊接工艺及焊后热处理制度是否满足设计规范对高温强度等指标的强制性要求,进而为构件在长期高温高压环境中的承载能力、变形稳定性与整体安全提供关键依据。
基于GB/T 228.2—2015《金属材料 拉伸试验 第2部分:高温试验方法》标准,在试板厚度中心T/2处及距上、下表面1.6 mm处分别制取高温拉伸试样,试样尺寸为⌀12.5 mm×110 mm,取样方向垂直于焊缝。详细试验结果见表7~表9,试样断裂形貌如图8所示。
为进一步考察焊缝材料本身在高温下的强度与塑性,在试板厚度中心(T/2)及距上、下表面1.6 mm处加工了全焊缝高温拉伸试样(尺寸为⌀12.5 mm×110 mm),试样方向平行于焊缝,试验结果见表10~表12。
在454 ℃高温条件下,依据12Cr2Mo1V钢加氢反应器相关技术文件及标准要求,其抗拉强度Rm≥461 MPa,屈服强度Rp0.2≥338 MPa。
通过焊接接头与全焊缝熔敷金属的高温拉伸试验,从整体与局部两个层面对焊接结构的高温安全性与可靠性进行了系统验证,取得了协同互补的评估效果。由表7~表12及图8可知,该焊接接头的高温拉伸性能稳定:其屈服强度与抗拉强度均不低于规定值,断后伸长率亦符合预期。所有试样均断裂于母材区域,焊缝及热影响区未出现破坏,这从力学性能上表明接头强度匹配合理、焊接质量可靠、工艺参数得当。试验过程严格遵循GB/T  228.2—2015及相关技术规范进行数据采集与结果评定。综上,该焊接接头的高温力学性能完全满足设计要求,结果良好。
通过开展-30  ℃低温冲击试验,研究12Cr2Mo1V钢焊接接头的低温韧性表现。焊接会引起热影响区组织变化(如形成粗晶区)并产生残余应力集中,导致该区域常出现韧性下降,成为低温脆性开裂的潜在危险区。为评价材料的断裂韧性并考察焊缝的韧性储备,试验选取-30  ℃作为测试温度,重点分析接头在韧脆转变温度附近的性能特征[10]。通过夏比V型缺口冲击吸收能量(KV2)的测量数据,结合断口纤维区比例的显微观察,综合评估接头在低温冲击下的能量吸收能力与抗裂纹扩展性。根据API RP 934-A—2019标准的要求,-30  ℃冲击试验结果应满足:3个试样冲击吸收能量平均值不低于54  J,且其中单个试样值不低于48  J。
从表13中-30  ℃冲击试验结果可知,各试样的冲击吸收能量均在130 J以上,远高于标准要求的54 J,表明接头低温冲击韧性良好,满足要求。
弯曲试验合格是焊接接头具有良好塑性、韧性及低缺陷率的直接证明。对12Cr2Mo1V钢焊接接头进行弯曲试验,可直观评估其整体(包括焊缝、熔合线及热影响区)的塑性变形能力与抗开裂性能,并能有效揭示潜在的焊接缺陷。
采用全厚度横向侧弯试样(10 mm×30 mm×200 mm),在弯曲半径20 mm、弯曲角度180°的规定条件下进行弯曲试验。如图9所示,弯曲后焊缝、熔合区及热影响区均未出现裂纹及其他缺陷。试验结果证明,该焊接接头具有良好的塑性变形能力和结构完整性,符合相关技术标准与规范要求。
12Cr2Mo1V钢焊接接头(尤其是热影响区中的粗晶区)长期处于400 ℃以上的复杂工况时,其组织状态(如原奥氏体晶粒尺寸和碳化物形态)以及杂质元素(如P,Sn,Sb,As等)的分布,均易引发回火脆化现象。通过回火脆化倾向评定试验,可有效评估该类钢材焊接接头在特定温度区间缓慢冷却或长期高温服役条件下,韧性显著下降(即产生回火脆性)的敏感性[11]。
该试验采用阶梯冷却工艺(见图10)模拟最为苛刻的脆化条件,通过对比处理前后焊缝与热影响区的低温冲击韧性,并以韧脆转变温度增量(ΔvTr54)作为关键评价指标,从而实现对焊接接头脆化敏感性的定量表征[12]。
根据API RP 934-A—2019,12Cr2Mo1V钢的回火脆化敏感性指标需满足vTr54+3ΔvTr54≤0 ℃的要求,且在316 ℃至593 ℃的加热过程中,加热速度为56 ℃/h。
其中,vTr54表示经最小焊后热处理后夏比V型缺口冲击吸收能量为54  J时所对应的韧脆转变温度(试验温度);ΔvTr54则表示在最小焊后热处理基础上再经阶梯冷却工艺处理后,冲击吸收能量同样达到54  J时所对应的转变温度增量。S.C表示阶梯冷却工艺;曲线A和曲线B分别为步冷前、后冲击吸收能量随试验温度变化的关系曲线。如图11所示,2条曲线各基于8个选定温度点绘制,每个温度点均测试3个夏比V型缺口冲击试样。
从表14中的试验结果可以看出,12Cr2Mo1V钢在回火脆化倾向试验中表现出优良的抗脆化能力,实测数据满足上述标准限值要求,表明该材料在实际高温服役条件下具备良好的韧性稳定性,能够符合相关技术文件对抗回火脆化性能的具体规定。
焊接过程中,水分、油污、焊条药皮或保护气体中的氢会溶入熔池,冷却后部分氢残留在金属晶格或微观缺陷内。这些可扩散氢在室温或升温条件下可逐渐迁移,并富集于应力集中区域(如显微缺陷或硬脆组织处)。一旦局部氢浓度达到临界值,且在残余应力共同作用下,易于诱发氢致裂纹[13]。
依据GB/T 3965—2012《熔敷金属中扩散氢测定方法》,采用热导法对12Cr2Mo1V钢焊接接头的扩散氢含量进行测定[14],从而定量评估焊接过程中渗入并残留于焊缝金属与热影响区内的可扩散氢含量,为判断和调控接头氢致延迟裂纹倾向提供依据。
经严格测定,本焊材熔敷金属的扩散氢含量实测结果(对应焊条电弧焊、单丝埋弧焊、双丝埋弧焊)依次为1.50,2.31,1.82 mL/100 g,显著优于设计与技术文件规定的不高于5 mL/100 g要求,证实该焊材为超低氢型,其品质能够满足高标准焊接的严苛需求。
为综合评价12Cr2Mo1V钢埋弧焊接头在模拟高温及长期应力耦合条件下的抗蠕变变形与断裂能力,依据GB/T 2039—2024《金属材料 单轴拉伸蠕变试验方法》开展高温持久强度试验[15]。根据该材料在压力容器中应用的相关技术规范及标准要求,试验在540 ℃,210  MPa恒定载荷下进行,要求持续承载时间不低于1 000  h。
表15示出T/2位置纵向全焊缝、T/2位置横向接头方向试样的高温持久强度测试结果。可以看出,该焊接接头的高温持久强度表现优异,实测数据完全满足12Cr2Mo1V钢技术标准中关于持久性能的各项指标要求,体现出良好的工程适用性与可靠性。
基于API RP 934-A—2019附录B对12Cr2Mo1V钢再热裂纹的相关分析,埋弧焊熔敷金属中若含有10-6级别的铅、铋等元素,可能引发焊缝再热裂纹[16]。再热裂纹敏感元素指标的计算公式如下:
Kf=Pb+Bi+0.03Sb
依据规范要求,Kf值应不大于1.5×10-6。采用热电XSeriesⅡ等离子质谱仪,对国产焊材的焊丝及熔敷金属进行Kf系数对比测试,结果如表16所示。可以看出,焊接过程中焊剂未额外引入与Kf系数相关的元素;熔敷金属的Kf系数略低于焊丝,说明部分有害元素在焊接过程中发生烧损,有利于提高焊缝质量,且所有测试结果均满足相关技术要求。
按API 934A附录B推荐的焊接参数制备埋弧焊丝熔敷金属拉伸试样,焊接参数为:电流550 A、电压31 V、焊接速度50 cm/min、层温≤230 ℃。在Gleeble热模拟拉伸试验机上开展热塑性拉伸试验,依据试验结果评价焊接材料的再热裂纹敏感性;规范要求2个试样的断面收缩率平均值不低于32%、单个试样断面收缩率不低于29%,满足该要求即认定其抗再热裂纹性能合格[17]。热塑性拉伸试验的试验条件及结果见表17。
综合熔敷金属Kf系数测试与高温慢拉伸试验结果,国产埋弧焊材的再热裂纹敏感性指标均符合技术要求,表现出较低的再热裂纹倾向。
结合上述试验结果及与进口焊材的多维度对比分析[18-19]可知,国产焊材在熔敷金属成分控制、低温冲击韧性及高温蠕变性能等方面均与进口产品相当,且其工艺操作性更适应国内生产条件,整体技术成熟度已达到国际先进水平。
基于上述试验结果,该国产焊材已成功应用于某百万吨乙烯项目炼油配套工程中2台大型加氢反应器的主体焊缝焊接。焊接过程中焊条药皮自动断裂性良好、脱渣顺畅,焊缝成形美观,工艺性能稳定,已实现批量化工业应用。所有焊缝经超声波衍射时差法(TOFD)、射线(RT)、超声(UT)及磁粉(MT)等无损检测方法综合评定,结果均符合设计要求;所附产品焊接试样的各项性能检测也全部满足设计要求。
根据该百万吨乙烯项目炼油配套工程中2台大型加氢反应器主焊缝的实际制造与检测反馈,所有焊缝的TOFD、RT及UT检测均一次合格,且焊缝中未超标缺陷的控制水平与同类进口焊材相当,部分指标甚至更优。
文中聚焦于12Cr2Mo1V钢制压力容器主焊缝焊接材料的国产化替代,通过系统的工艺评定与性能测试,验证了国产焊材在关键性能与工艺适用性方面的可靠性。主要结论如下:
(1)采用国产焊材施焊所得的焊接接头成型质量均优异,焊缝表面均匀规整,未观察到气孔、裂纹等宏观缺陷。
(2)理化性能测试结果表明,该焊接接头的综合性能完全满足12Cr2Mo1V钢制加氢反应器的相关技术要求。
(3)在相同工艺条件下,无损检测(TOFD/RT/UT)结果表明,采用国产焊材的焊缝质量表现优异,其未超标缺陷的控制能力与进口焊材相当,部分指标甚至更优,实现了对同类进口焊材的质量超越。

参考文献 引证文献
排序方式:
1
蒋军,房务农.我国压力容器用高端焊接材料国产化现状及发展趋势[J].金属加工(热加工),2020(6):19-24.
JIANG J,FANG W N.Current status and development trend of localization of high‑end welding materials for pressure vessels[J].MW Metal Forming,2020(6):19-24.
2
张颖,尚尔晶,谷文.2.25Cr-1Mo和2.25Cr-1Mo-0.25V钢加氢反应器材料和制造经验[J].压力容器,2014,31(12):73-78.
ZHANG Y,SHANG E J,GU W.Materials and fabrication experience of 2.25Cr-1Mo and 2.25Cr-1Mo-0.25V steel hydrogenation reactor[J].Pressure Vessel Technology,2014,31(12):73-78.
3
陈晓玲,李多民,段滋华.加氢反应器的发展现状[J].化工装备技术,2009,30(1):28-31.
CHEN X L,LI D M,DUAN Z H.Development status of hydrogenation reactor[J].Chemical Equipment Technology,2009,30(1):28-31.
4
王雪骄,范阳阳,晏君文,等.2.25Cr-1Mo-0.25V钢上国产焊材单层带极堆焊工艺研究[J].大型铸锻件,2023(5):32-36.
WANG X J,FAN Y Y,YAN J W,et al.Research on the technology of single‑layered strip surfacing on 2.25Cr-1Mo-0.25V steel with domestic welding materials[J].Heavy Casting and Forging,2023(5):32-36.
5
王小刚.2.25Cr-1Mo-0.25V钢埋弧焊焊材及熔敷金属组织性能研究[D].北京:机械科学研究总院,2006.
WANG X G.Study on the submerged arc welding consumables for 2.25Cr-1Mo-0.25V steel and its microstructure and mechanical properties of the deposited metal[D].Beijing:Academy of Machinery Science & Technology,2006.
6
魏艳红,张修智,杜文,等.焊接接头机械性能预测专家系统——PPES[J].焊接学报,1993(4):268-272.
WEI Y H,ZHANG X Z,DU W,et al.Expert system for predicting mechanical properties of welded joints—PPES[J].Transactions of the China Welding Institution,1993(4):268-272.
7
汪建华,陆皓.焊接残余应力形成机制与消除原理若干问题的讨论[J].焊接学报,2002(3):75-79.
WANG J H,LU H.Some discussions on principle of causing and relieving welding residual stress[J].Transactions of the China Welding Institution,2002(3):75-79.
8
薛巍,李南,党兆凯.2.25Cr-1Mo-0.25V钢板热处理工艺试验[J].压力容器,2004,21(10):10-13.
XUE W,LI N,DANG Z K.Test on heat treatment of 2.25Cr-1Mo-0.25V steel plate[J].Pressure Vessel Technology,2004,21(10):10-13.
9
张敏,徐蔼彦,汪强,等.高温运行后12Cr1MoV钢焊接接头的显微组织和力学性能[J].机械工程材料,2016,40(2):98-101.
ZHANG M,XU A Y,WANG Q,et al.Microstructure and mechanical properties of 12Cr1MoV steel welded joint after high temperature service[J].Materials for Mechanical Engineering,2016,40(2):98-101.
10
马窦琴,宋亚虎,赵学谦,等.加氢锻件用2.25Cr-1Mo-0.25V钢的冲击韧性[J].材料科学与工程学报,2020,38(4):625-628.
MA D Q,SONG Y H,ZHAO X Q,et al.Research on impact toughness of 2.25Cr-1Mo-0.25V steel for hydrogenation forgings[J].Journal of Materials Science and Engineering,2020,38(4):625-628.
11
柯杨,刘仕伟.压力容器材料韧脆转变温度曲线拟合分析及应用研究[J].冶金与材料,2019,39(5):60-61.
KE Y,LIU S W.Curve fitting analysis and application research on ductile-brittle transition temperature of pressure vessel materials[J].Metallurgy and Materials,2019,39(5):60-61.
12
马韩韩,伏玮,沈志鹏,等.基于步冷试验的2.25Cr-1Mo-0.25V钢母材及焊缝回火脆化研究[J].压力容器,2020,37(2):1-10.
MA H H,FU W,SHEN Z P,et al.Study on temper embrittlement of 2.25Cr-1Mo-0.25V steel base metal and welded joint based on step‑cooling test[J].Pressure Vessel Technology,2020,37(2):1-10.
13
张敬强.焊接接头中应力促进氢致裂纹形成理论分析与实验研究[D].哈尔滨:哈尔滨工业大学,2015.
ZHANG J Q.Theoretical analysis and experimental research on stress‑facilitated nucleation of hydrogen induced cracking in welded joint[D].Harbin:Harbin Institute of Technology,2015.
14
宗杰,蒋志强.熔敷金属中扩散氢含量的测定[J].理化检验(物理分册),2017,53(12):879-881.
ZONG J,JIANG Z Q.Determination of diffusible hydrogen content in deposited metals[J].Physical Testing and Chemical Analysis(Part A:Physical Testing),2017,53(12):879-881.
15
武欣宇.2.25Cr1MoV钢加氢反应设备蠕变疲劳寿命设计方法[D].天津:天津大学,2015.
WU X Y.A design approach for creep fatigue evaluation of hydrogenation reactor made of 2.25Cr1MoV steel[J].Tianjin:Tianjin University,2015.
16
韩一纯.2.25Cr1Mo0.25V钢再热裂纹生成机理研究[D].合肥:中国科学技术大学,2015.
HAN Y C.Study on the mechanism of reheat cracking in 2.25Cr1Mo0.25V steel[D].Hefei:University of Science and Technology of China,2015.
17
卜华全,任明皓,姜恒.Gleeble试验中再热裂纹敏感性评价方法探讨[J].压力容器,2019,36(11):1-5.
BO H Q,REN M H,JIANG H.Discussion on evaluation method of reheat crack sensitivity in gleeble test[J].Pressure Vessel Technology,2019,36(11):1-5.
18
王雪骄,何鹏,晏君文,等.12Cr2Mo1V钢凸台附加填充丝埋弧堆焊工艺研究[J]. 压力容器,2024,41(4):16-21.
WANG X J,HE P,YAN J W,et al.Research of submerged arc welding build up technology of 12Cr2Mo1V steel boss using additional filing wire[J].Pressure Vessel Technology,2024,41(4):16-21.
19
秦牧,程光旭,李青,等.2.25Cr-1Mo-0.25V钢加氢反应器焊接接头的性能影响因素研究[J].压力容器,2022,39(3):9-18.
QIN M,CHENG G X,LI Q,et al.Study of influence factors on quality of 2.25Cr-1Mo-0.25V steel for welded joint of hydrogenation reactor[J].Pressure Vessel Technology,2022,39(3):9-18.
2025年第42卷第11期
135
64
0
引用本文
BibTeX
文章信息
doi: 10.3969/j.issn.1001-4837.2025.11.002
  • 接收时间:2025-09-22
  • 首发时间:2026-11-11
  • 出版时间:2025-11-30
补充材料
相关文章
文章信息
作者
出版历史
  • 收稿日期:2025-09-22
  • 修回日期:2025-10-23
基金
作者信息
    1二重(德阳)重型装备有限公司,四川 德阳 618000
    2四川西冶新材料股份有限公司,成都 610000
参考文献
分享链接
https://castjournals.cast.org.cn/joweb/ylrq/CN/10.3969/j.issn.1001-4837.2025.11.002
分享至
全文二维码

扫描看全文

引用本文
BibTeX
本文的引用情况
2种不同金属材料的力学参数
科
Family
属数
Number of
genus
种数
Number of
species
占总种数比例
Percentage of
total species (%)
属
Genus
种数
Number of
species
占总种数比例
Percentage of total
species (%)
鹅膏菌科Amanitaceae 2 11 5.26 鹅膏菌属 Amanita 10 4.78
小菇科 Mycenaceae 2 12 5.74 丝盖伞属 Inocybe 5 2.39
多孔菌科 Polyporaceae 8 14 6.70 蜡蘑属 Laccaria 5 2.39
红菇科 Russulaceae 3 23 11.00 小皮伞属 Marasmius 6 2.87
小菇属 Mycena 11 5.26
光柄菇属 Pluteus 5 2.39
红菇属 Russula 17 8.13
栓菌属 Trametes 5 2.39
关闭全屏