Article(id=1324796175555100911, tenantId=1146029695717560320, journalId=1319355204128309394, issueId=1324796014586114936, articleNumber=null, orderNo=null, doi=10.3969/j.issn.1001-4837.2025.06.003, pmid=null, cstr=null, oa=null, hot=null, price=null, onlineType=0, articleFormat=0, articleType=null, articleTypeStr=null, receivedDate=1735747200000, receivedDateStr=2025-01-02, revisedDate=1745337600000, revisedDateStr=2025-04-23, acceptedDate=null, acceptedDateStr=null, onlineDate=1793785621774, onlineDateStr=2026-11-04, pubDate=1751212800000, pubDateStr=2025-06-30, doiRegisterDate=null, doiRegisterDateStr=null, onlineIssueDate=1793785621774, onlineIssueDateStr=2026-11-04, onlineJustAcceptDate=null, onlineJustAcceptDateStr=null, onlineFirstDate=null, onlineFirstDateStr=null, sourceXml=null, magXml=null, createTime=1793785621774, creator=13701087609, updateTime=1793785621774, updator=13701087609, issue=Issue{id=1324796014586114936, tenantId=1146029695717560320, journalId=1319355204128309394, year='2025', volume='42', issue='6', pageStart='1', pageEnd='81', issueExtLink='null', onlineDate='null', pubDate='1751212800000', pubDateStr='2025-06-30', beforeIssueId=null, nextIssueId=null, price=null, status=1, issueComplete=1, articleOrder=1, issueType=-1, specialIssue=null, createTime=1793785583397, creator='13701087609', updateTime=1793787536357, updator='13701087609', preIssue=null, nextIssue=null, articleTotal=null, ext={EN=IssueExt(id=1324804205969552288, tenantId=1146029695717560320, journalId=1319355204128309394, issueId=1324796014586114936, language=EN, specialIssueTitle=, coverIllustrator=null, specialIssueEditor=, specialIssueAbout=), CN=IssueExt(id=1324804205969552289, tenantId=1146029695717560320, journalId=1319355204128309394, issueId=1324796014586114936, language=CN, specialIssueTitle=, coverIllustrator=null, specialIssueEditor=, specialIssueAbout=)}, issueFiles=null, downloadFileDto=null}, startPage=19, endPage=24, ext={EN=ArticleExt(id=1324796175743844592, articleId=1324796175555100911, tenantId=1146029695717560320, journalId=1319355204128309394, language=EN, title=Research and application of TP316L stainless steel cladding process on 20MnNiMo steel surface, columnId=1320422992476226524, journalTitle=Pressure Vessel Technology, columnName=Experimental Researches, runingTitle=null, highlight=null, articleAbstract=

To address the insufficient corrosion resistance of 20MnNiMo steel in specific environments,three welding processes,electroslag welding (ESW),flux cored arc welding (FCAW),and gas tungsten arc welding (GTAW),were employed to overlay a TP316L stainless steel layer on its surface to improve corrosion resistance.Stable welding parameters were determined through welding process tests,and the cladding layers were subjected to chemical composition analysis,side bend tests,hardness tests,intergranular corrosion tests,and metallographic structure observation.The results indicate that the chemical composition of the cladding layers is uniform and meets standard requirements(Ni mass fraction:11.0% to 15.0%,Cr mass fraction:16.0% to 20.0%);no cracks were generated in the side bend tests;hardness values were all below 250HV10;intergranular corrosion performance was qualified;and the microstructure consisted of a uniform austenitic matrix with a small amount of ferrite.The study confirms that all three processes,ESW,FCAW,and GTAW,can meet equipment manufacturing requirements.ESW uses single layer strip cladding with a cladding thickness of 4.0 to 4.5 mm;FCAW and GTAW require a two layer cladding of transition layer TP309L and corrosion resistant layer TP316L,with at least one layer for FCAW and at least two layers for GTAW in the corrosion resistant layer,and a total cladding thickness of 5.0 to 5.5 mm.This research provides reliable data support and process guidance for the engineering application of 20MnNiMo steel in corrosive environments,demonstrating significant practical engineering value.

, authors=Xuejiao WANG, authorsList=Xuejiao WANG, authorCompany=null, correspAuthors=null, authorNote=null, correspAuthorsNote=null, copyrightStatement=null, copyrightOwner=null, extLink=null, articleAbsUrl=null, sourceXml=null, magXml=null, pdfUrl=null, pdf=null, pdfFileSize=null, pdfExtLink=null, richHtmlUrl=null, mobilePdfUrl=null, reviewReport=null, pdfFirstPage=null, abstractGraph=null, abstractGraphContent=null, abstractVideo=null, citation=null, cebUrl=null, magXmlContent=null, mapNumber=null, fund=null), CN=ArticleExt(id=1324796178314952951, articleId=1324796175555100911, tenantId=1146029695717560320, journalId=1319355204128309394, language=CN, title=20MnNiMo钢表面TP316L不锈钢堆焊工艺研究及应用, columnId=1320422992698524638, journalTitle=压力容器, columnName=试验研究, runingTitle=null, highlight=null, articleAbstract=

针对20MnNiMo钢在特定环境下的耐腐蚀性能不足问题,采用电渣焊(ESW)、药芯焊丝电弧焊(FCAW)和钨极气体保护焊(GTAW) 3种工艺,在其表面堆焊TP316L不锈钢层以提高其耐蚀性。通过焊接工艺试验确定了稳定的焊接参数,并对堆焊层进行了化学成分分析、侧弯试验、硬度测试、晶间腐蚀试验及金相组织观察。结果表明,堆焊层化学成分均匀,且符合标准要求(Ni的质量分数为11.0%~15.0%,Cr的质量分数为16.0%~20.0%);侧弯试验无裂纹产生;硬度值均低于250HV10;晶间腐蚀性能合格;显微组织为均匀的奥氏体基体+少量铁素体。研究证实,ESW,FCAW和GTAW 3种工艺均能满足设备制造要求,ESW采用单层带极堆焊,堆焊层厚度4.0~4.5 mm;FCAW和GTAW堆焊时需采用过渡层TP309L+耐蚀层TP316L双层堆焊,耐蚀层FCAW至少1层,耐蚀层GTAW至少2层,堆焊层总厚度5.0~5.5 mm。该研究为20MnNiMo钢在腐蚀环境中的工程应用提供了可靠的数据支撑和工艺指导,具有重要的工程实践价值。

, authors=王雪骄, authorsList=王雪骄, authorCompany=null, correspAuthors=null, authorNote=

王雪骄(1978),女,正高级工程师,主要从事压力容器焊接制造技术的研究与开发工作,通信地址:618000四川省德阳市二重(德阳)重型装备有限公司重型压力容器及核电技术研究所,E-mail:。

, correspAuthorsNote=null, copyrightStatement=作者向本刊所投稿件一经本刊录用,则该论文的复制权、发行权、信息网络传播权、翻译权、汇编权等权利视为自动转让给本刊。本刊为国内各主要数据库收录期刊,本刊所发表的稿件将同时通过因特网进行网络出版或提供信息服务(包括印刷版、光盘版和网络版等各种使用方式)。, copyrightOwner=null, extLink=null, articleAbsUrl=null, sourceXml=IK5bKBpdUl2qet8c2QaUEw==, magXml=Wh2SEqmYKxlRmyltxaJ8cA==, pdfUrl=null, pdf=n7r1SNIK+HgSIB0XafDiqg==, pdfFileSize=1721243, pdfExtLink=null, richHtmlUrl=null, mobilePdfUrl=null, reviewReport=null, pdfFirstPage=null, abstractGraph=GfXaqeY5GK0gV162BMy6Qw==, abstractGraphContent=null, abstractVideo=null, citation=null, cebUrl=null, magXmlContent=UGlkhuzXXc6BDaFrRJpKVg==, mapNumber=null, fund=null)}, authors=[Author(id=1324796178667274492, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, orderNo=0, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=NN791H528@163.com, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1324796178738577662, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, authorId=1324796178667274492, language=EN, stringName=Xuejiao WANG, firstName=Xuejiao, middleName=null, lastName=WANG, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1324796178826658047, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, authorId=1324796178667274492, language=CN, stringName=王雪骄, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=1二重(德阳)重型装备有限公司,四川 德阳 618000, bio={"content":"

王雪骄(1978),女,正高级工程师,主要从事压力容器焊接制造技术的研究与开发工作,通信地址:618000四川省德阳市二重(德阳)重型装备有限公司重型压力容器及核电技术研究所,E-mail:。

"}, bioImg=null, bioContent=

王雪骄(1978),女,正高级工程师,主要从事压力容器焊接制造技术的研究与开发工作,通信地址:618000四川省德阳市二重(德阳)重型装备有限公司重型压力容器及核电技术研究所,E-mail:。

, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1324796178545639672, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, xref=1, ext=[AuthorCompanyExt(id=1324796178554028281, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, companyId=1324796178545639672, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China), AuthorCompanyExt(id=1324796178566611194, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, companyId=1324796178545639672, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1二重(德阳)重型装备有限公司,四川 德阳 618000)])])], keywords=[Keyword(id=1324796178935709952, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=EN, orderNo=1, keyword=20MnNiMo steel), Keyword(id=1324796178998624513, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=EN, orderNo=2, keyword=TP316L steel), Keyword(id=1324796179057344770, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=EN, orderNo=3, keyword=electroslag welding), Keyword(id=1324796179124453635, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=EN, orderNo=4, keyword=flux cored arc welding), Keyword(id=1324796179183173892, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=EN, orderNo=5, keyword=gas tungsten arc welding), Keyword(id=1324796179246088453, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=CN, orderNo=1, keyword=20MnNiMo钢), Keyword(id=1324796179309003014, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=CN, orderNo=2, keyword=TP316L钢), Keyword(id=1324796179367723271, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=CN, orderNo=3, keyword=电渣焊), Keyword(id=1324796179443220744, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=CN, orderNo=4, keyword=药芯焊丝电弧焊), Keyword(id=1324796179506135305, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=CN, orderNo=5, keyword=钨极气体保护焊)], refs=[Reference(id=1324796181125136670, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2016, volume=39, issue=6, pageStart=1, pageEnd=4, url=null, language=null, rfNumber=1, rfOrder=0, authorNames=王强, 麻永林, 陈重毅, journalName=山西冶金, refType=null, unstructuredReference=王强,麻永林,陈重毅,等.焊接热输入对厚壁20MnNiMo钢焊缝性能的影响[J].山西冶金,2016,39(6):1-4., articleTitle=焊接热输入对厚壁20MnNiMo钢焊缝性能的影响, refAbstract=null), Reference(id=1324796182718972191, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2016, volume=39, issue=6, pageStart=1, pageEnd=4, url=null, language=null, rfNumber=1, rfOrder=1, authorNames=WANG Q, MA Y L, CHEN Z Y, journalName=Shanxi Metallurgy, refType=null, unstructuredReference=WANG Q,MA Y L,CHEN Z Y,et al.Effect of welding heat input on properties of weld seam of thick 20MnNiMo steel[J].Shanxi Metallurgy,2016,39(6):1-4., articleTitle=Effect of welding heat input on properties of weld seam of thick 20MnNiMo steel, refAbstract=null), Reference(id=1324796182798663968, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2013, volume=34, issue=1, pageStart=76, pageEnd=80, url=null, language=null, rfNumber=2, rfOrder=2, authorNames=陈重毅, 麻永林, 邢淑清, journalName=材料热处理学报, refType=null, unstructuredReference=陈重毅,麻永林,邢淑清,等.焊接热输入对特厚板20MnNiMo焊接残余应力的影响[J].材料热处理学报,2013,34(1):76-80., articleTitle=焊接热输入对特厚板20MnNiMo焊接残余应力的影响, refAbstract=null), Reference(id=1324796183020962081, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2013, volume=34, issue=1, pageStart=76, pageEnd=80, url=null, language=null, rfNumber=2, rfOrder=3, authorNames=CHEN Z Y, MA Y L, XING S Q, journalName=Transactions of Materials and Heat Treatment, refType=null, unstructuredReference=CHEN Z Y,MA Y L,XING S Q,et al.Effect of welding heat input on welding residual stress in submerged‑arc welds of thick plate 20MnNiMo joints[J].Transactions of Materials and Heat Treatment,2013,34(1):76-80., articleTitle=Effect of welding heat input on welding residual stress in submerged‑arc welds of thick plate 20MnNiMo joints, refAbstract=null), Reference(id=1324796183385866530, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2012, volume=33, issue=4, pageStart=96, pageEnd=99, url=null, language=null, rfNumber=3, rfOrder=4, authorNames=迟露鑫, 陈重毅, 麻永林, journalName=材料热处理学报, refType=null, unstructuredReference=迟露鑫,陈重毅,麻永林,等.焊后热处理对特厚板 20MnNiMo焊接残余应力的影响[J].材料热处理学报,2012,33(4):96-99., articleTitle=焊后热处理对特厚板 20MnNiMo焊接残余应力的影响, refAbstract=null), Reference(id=1324796183478141219, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2012, volume=33, issue=4, pageStart=96, pageEnd=99, url=null, language=null, rfNumber=3, rfOrder=5, authorNames=CHI L X, CHEN Z Y, MA Y L, journalName=Transactions of Materials and Heat Treatment, refType=null, unstructuredReference=CHI L X,CHEN Z Y,MA Y L,et al.Effect of post‑weld heat treatment on residual stress in submerged‑arc welds of 20MnNiMo steel heavy plate [J].Transactions of Materials and Heat Treatment,2012,33(4):96-99., articleTitle=Effect of post‑weld heat treatment on residual stress in submerged‑arc welds of 20MnNiMo steel heavy plate, refAbstract=null), Reference(id=1324796183884988708, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2000, volume=21, issue=1, pageStart=9, pageEnd=12, url=null, language=null, rfNumber=4, rfOrder=6, authorNames=张显辉, 焦伟, 谭长瑛, journalName=焊接学报, refType=null, unstructuredReference=张显辉,焦伟,谭长瑛.20MnNiMo钢焊接热影响区的组织和韧性及其氢致裂纹特征[J].焊接学报,2000,21(1):9-12., articleTitle=20MnNiMo钢焊接热影响区的组织和韧性及其氢致裂纹特征, refAbstract=null), Reference(id=1324796184220533029, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2000, volume=21, issue=1, pageStart=9, pageEnd=12, url=null, language=null, rfNumber=4, rfOrder=7, authorNames=ZHANG X H, JIAO W, TAN C Y, journalName=Transactions of the China Welding Institution, refType=null, unstructuredReference=ZHANG X H,JIAO W,TAN C Y.HAZ structure,toughness and characteristics to hydrogen‑induced cracking(HIC) of steel 20MnNiMo[J].Transactions of the China Welding Institution,2000,21(1):9-12., articleTitle=HAZ structure,toughness and characteristics to hydrogen‑induced cracking(HIC) of steel 20MnNiMo, refAbstract=null), Reference(id=1324796184287641894, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2002, volume=23, issue=3, pageStart=23, pageEnd=25, url=null, language=null, rfNumber=5, rfOrder=8, authorNames=张显辉, 焦伟, 谭长瑛, journalName=焊接学报, refType=null, unstructuredReference=张显辉,焦伟,谭长瑛.20MnNiMo钢焊接氢致裂纹特征(Ⅱ)[J].焊接学报,2002,23(3):23-25., articleTitle=20MnNiMo钢焊接氢致裂纹特征(Ⅱ), refAbstract=null), Reference(id=1324796184363139367, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2002, volume=23, issue=3, pageStart=23, pageEnd=25, url=null, language=null, rfNumber=5, rfOrder=9, authorNames=ZHANG X H, JIAO W, TAN C Y, journalName=Transactions of the China Welding Institution, refType=null, unstructuredReference=ZHANG X H,JIAO W,TAN C Y.Hydrogen‑induced cracking feature of steel 20MnNiMo(Ⅱ)[J].Transactions of the China Welding Institution,2002,23(3):23-25., articleTitle=Hydrogen‑induced cracking feature of steel 20MnNiMo(Ⅱ), refAbstract=null), Reference(id=1324796184438636840, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2009, volume=null, issue=12, pageStart=25, pageEnd=29, url=null, language=null, rfNumber=6, rfOrder=10, authorNames=刘玉华, journalName=金属加工(热加工), refType=null, unstructuredReference=刘玉华.CO2药芯焊丝气保焊(FCAW)在加氢反应器接管内壁不锈钢堆焊中的应用[J].金属加工(热加工),2009(12):25-29., articleTitle=CO2药芯焊丝气保焊(FCAW)在加氢反应器接管内壁不锈钢堆焊中的应用, refAbstract=null), Reference(id=1324796184690295081, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2009, volume=null, issue=12, pageStart=25, pageEnd=29, url=null, language=null, rfNumber=6, rfOrder=11, authorNames=LIU Y H, journalName=MW Metal Forming, refType=null, unstructuredReference=LIU Y H.Application of CO2 flux‑cored wire arc welding (FCAW) in stainless steel surfacing on the inner wall of hydrogenation reactor nozzle[J].MW Metal Forming,2009(12):25-29., articleTitle=Application of CO2 flux‑cored wire arc welding (FCAW) in stainless steel surfacing on the inner wall of hydrogenation reactor nozzle, refAbstract=null), Reference(id=1324796184769986858, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2021, volume=null, issue=5, pageStart=28, pageEnd=31, url=null, language=null, rfNumber=7, rfOrder=12, authorNames=王晖球, 王雪骄, 叶小松, journalName=大型铸锻件, refType=null, unstructuredReference=王晖球,王雪骄,叶小松.国产不锈钢双电渣堆焊材料在加钒钢加氢反应器上的应用[J].大型铸锻件,2021(5):28-31., articleTitle=国产不锈钢双电渣堆焊材料在加钒钢加氢反应器上的应用, refAbstract=null), Reference(id=1324796184845484331, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2021, volume=null, issue=5, pageStart=28, pageEnd=31, url=null, language=null, rfNumber=7, rfOrder=13, authorNames=WANG H Q, WANG X J, YE X S, journalName=Heavy Casting and Forging, refType=null, unstructuredReference=WANG H Q,WANG X J,YE X S.Application of domestic stainless steel double‑layer electro‑slag surfacing on the vanadium steel hydrogenation reactor[J].Heavy Casting and Forging,2021(5):28-31., articleTitle=Application of domestic stainless steel double‑layer electro‑slag surfacing on the vanadium steel hydrogenation reactor, refAbstract=null), Reference(id=1324796185151668524, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2024, volume=41, issue=11, pageStart=74, pageEnd=84, url=null, language=null, rfNumber=8, rfOrder=14, authorNames=邢卓, journalName=压力容器, refType=null, unstructuredReference=邢卓.管板带极电渣堆焊双相不锈钢工艺[J].压力容器,2024,41(11):74-84., articleTitle=管板带极电渣堆焊双相不锈钢工艺, refAbstract=null), Reference(id=1324796185487212845, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2024, volume=41, issue=11, pageStart=74, pageEnd=84, url=null, language=null, rfNumber=8, rfOrder=15, authorNames=XING Z, journalName=Pressure Vessel Technology, refType=null, unstructuredReference=XING Z.Overview of surfacing duplex stainless steel on tubesheets by electroslag strip welding[J].Pressure Vessel Technology,2024,41(11):74-84., articleTitle=Overview of surfacing duplex stainless steel on tubesheets by electroslag strip welding, refAbstract=null), Reference(id=1324796185558516014, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2011, volume=28, issue=11, pageStart=41, pageEnd=46, url=null, language=null, rfNumber=9, rfOrder=16, authorNames=陈志林, 刘应虎, journalName=压力容器, refType=null, unstructuredReference=陈志林,刘应虎.90 mm宽带极堆焊奥氏体不锈钢的化学成分及铁素体FN分析[J].压力容器,2011,28(11):41-46., articleTitle=90 mm宽带极堆焊奥氏体不锈钢的化学成分及铁素体FN分析, refAbstract=null), Reference(id=1324796187236237615, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2011, volume=28, issue=11, pageStart=41, pageEnd=46, url=null, language=null, rfNumber=9, rfOrder=17, authorNames=CHEN Z L, LIU Y H, journalName=Pressure Vessel Technology, refType=null, unstructuredReference=CHEN Z L,LIU Y H.Chemical elements and ferrite number analysis of austenitic stainless steel surfacing process with 90 mm strip electrode[J].Pressure Vessel Technology,2011,28(11):41-46., articleTitle=Chemical elements and ferrite number analysis of austenitic stainless steel surfacing process with 90 mm strip electrode, refAbstract=null), Reference(id=1324796187609530672, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2023, volume=null, issue=5, pageStart=32, pageEnd=36, url=null, language=null, rfNumber=10, rfOrder=18, authorNames=王雪骄, 范阳阳, 晏君文, journalName=大型铸锻件, refType=null, unstructuredReference=王雪骄,范阳阳,晏君文,等.2.25Cr-1Mo-0.25V钢上国产焊材单层带极电渣堆焊工艺研究[J].大型铸锻件,2023(5):32-36., articleTitle=2.25Cr-1Mo-0.25V钢上国产焊材单层带极电渣堆焊工艺研究, refAbstract=null), Reference(id=1324796187680833841, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2023, volume=null, issue=5, pageStart=32, pageEnd=36, url=null, language=null, rfNumber=10, rfOrder=19, authorNames=WANG X J, FAN Y Y, YAN J W, journalName=Heavy Casting and Forging, refType=null, unstructuredReference=WANG X J,FAN Y Y,YAN J W,et al.The technology study of single‑layer ESW cladding on 2.25Cr-1Mo-0.25V steel surface using domestic welding materials[J].Heavy Casting and Forging,2023(5):32-36., articleTitle=The technology study of single‑layer ESW cladding on 2.25Cr-1Mo-0.25V steel surface using domestic welding materials, refAbstract=null), Reference(id=1324796188075098418, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2016, volume=33, issue=3, pageStart=61, pageEnd=68, url=null, language=null, rfNumber=11, rfOrder=20, authorNames=王雪骄, 王迎君, 晏君文, journalName=压力容器, refType=null, unstructuredReference=王雪骄,王迎君,晏君文,等.加氢反应器E309L过渡层经PWHT后堆焊或焊接E347对基体材料的影响[J].压力容器,2016,33(3):61-68., articleTitle=加氢反应器E309L过渡层经PWHT后堆焊或焊接E347对基体材料的影响, refAbstract=null), Reference(id=1324796188138012979, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, doi=null, pmid=null, pmcid=null, year=2016, volume=33, issue=3, pageStart=61, pageEnd=68, url=null, language=null, rfNumber=11, rfOrder=21, authorNames=WANG X J, WANG Y J, YAN J W, journalName=Pressure Vessel Technology, refType=null, unstructuredReference=WANG X J,WANG Y J,YAN J W,et al.Influence of welding or cladding E347 on E309L transition layer after PWHT to substrate material in hydrogenation reactor[J].Pressure Vessel Technology,2016,33(3):61-68., articleTitle=Influence of welding or cladding E347 on E309L transition layer after PWHT to substrate material in hydrogenation reactor, refAbstract=null)], funds=null, companyList=[AuthorCompany(id=1324796178545639672, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, xref=1, ext=[AuthorCompanyExt(id=1324796178554028281, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, companyId=1324796178545639672, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China), AuthorCompanyExt(id=1324796178566611194, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, companyId=1324796178545639672, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1二重(德阳)重型装备有限公司,四川 德阳 618000)])], figs=[ArticleFig(id=1324796179619381514, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=EN, label=Fig.1, caption=Dimensions of large and small side bend specimens, figureFileSmall=fDNdiuc5eq7o5h/EvLh7fA==, figureFileBig=GfXaqeY5GK0gV162BMy6Qw==, tableContent=null), ArticleFig(id=1324796179682296075, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=CN, label=图1, caption=大、小侧弯试样尺寸

备注1:当试件(含堆焊层)厚度小于试样宽度标注尺寸时,试样宽度为试件(含堆焊层)厚度。

, figureFileSmall=fDNdiuc5eq7o5h/EvLh7fA==, figureFileBig=GfXaqeY5GK0gV162BMy6Qw==, tableContent=null), ArticleFig(id=1324796179850068236, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=EN, label=Fig.2, caption=Cladding layer hardness test data, figureFileSmall=9kkNLhpm9ke0lHxY8IyNcw==, figureFileBig=REM5VN/oKqGm7IpqQQ8JtQ==, tableContent=null), ArticleFig(id=1324796179917177101, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=CN, label=图2, caption=堆焊层硬度检测数据, figureFileSmall=9kkNLhpm9ke0lHxY8IyNcw==, figureFileBig=REM5VN/oKqGm7IpqQQ8JtQ==, tableContent=null), ArticleFig(id=1324796179975897358, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=EN, label=Fig.3, caption=Microstructure 200×, figureFileSmall=8HL1vOm2bdqH5l/qv3F8Lg==, figureFileBig=kzDCKJNAdzj/uvlFgLj6mg==, tableContent=null), ArticleFig(id=1324796180034617615, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=CN, label=图3, caption=微观金相组织 200×

(a)ESW  (b)FCAW  (c)GTAW

, figureFileSmall=8HL1vOm2bdqH5l/qv3F8Lg==, figureFileBig=kzDCKJNAdzj/uvlFgLj6mg==, tableContent=null), ArticleFig(id=1324796180093337872, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=EN, label=Tab.1, caption=

Chemical composition requirements of cladding layer

, figureFileSmall=null, figureFileBig=null, tableContent=
化学元素CMnSiPSNiCrMoCu
含量≤0.04≤2.5≤1.00≤0.030≤0.02011.0~15.016.0~20.02.0~3.0≤0.75
), ArticleFig(id=1324796180156252433, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=CN, label=表1, caption=

堆焊层化学成分要求

, figureFileSmall=null, figureFileBig=null, tableContent=
化学元素CMnSiPSNiCrMoCu
含量≤0.04≤2.5≤1.00≤0.030≤0.02011.0~15.016.0~20.02.0~3.0≤0.75
), ArticleFig(id=1324796180219166994, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=EN, label=Tab.2, caption=

Chemical composition of 20MnNiMo steel

, figureFileSmall=null, figureFileBig=null, tableContent=
化学元素CSiMnPSCrMo
要求值0.17~0.230.15~0.401.20~1.50≤0.012≤0.005≤0.300.45~0.60
实测值0.200.251.310.0060.0010.180.50
化学元素NiVAsSnSbPbBi
要求值0.40~1.00≤0.050<0.015<0.015<0.010<0.010<0.010
实测值0.430.0030.0060.0030.0010.0010.001
化学元素As+Sn+Sb+Pb+BiH(0.001‰)O(0.001‰)N(0.001‰)Cu—
要求值<0.035提供数据≤0.20—
实测值0.0120.613500.06—
), ArticleFig(id=1324796180286275859, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=CN, label=表2, caption=

20MnNiMo钢的化学成分

, figureFileSmall=null, figureFileBig=null, tableContent=
化学元素CSiMnPSCrMo
要求值0.17~0.230.15~0.401.20~1.50≤0.012≤0.005≤0.300.45~0.60
实测值0.200.251.310.0060.0010.180.50
化学元素NiVAsSnSbPbBi
要求值0.40~1.00≤0.050<0.015<0.015<0.010<0.010<0.010
实测值0.430.0030.0060.0030.0010.0010.001
化学元素As+Sn+Sb+Pb+BiH(0.001‰)O(0.001‰)N(0.001‰)Cu—
要求值<0.035提供数据≤0.20—
实测值0.0120.613500.06—
), ArticleFig(id=1324796180349190420, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=EN, label=Tab.3, caption=

Mechanical properties of 20MnNiMo steel

, figureFileSmall=null, figureFileBig=null, tableContent=
项目热处理状态要求值实测值
Rm/MPaMax.PWHT620~790672
ReL/MPa≥450542
A/%≥1623.0
KV2(-20 ℃)/JMin.PWHT≥47214,229,228
冷弯D=3a,无裂纹无裂纹
硬度/HBW提供数据215,220,222
), ArticleFig(id=1324796180412104981, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=CN, label=表3, caption=

20MnNiMo钢的力学性能

, figureFileSmall=null, figureFileBig=null, tableContent=
项目热处理状态要求值实测值
Rm/MPaMax.PWHT620~790672
ReL/MPa≥450542
A/%≥1623.0
KV2(-20 ℃)/JMin.PWHT≥47214,229,228
冷弯D=3a,无裂纹无裂纹
硬度/HBW提供数据215,220,222
), ArticleFig(id=1324796180479213846, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=EN, label=Tab.4, caption=

Chemical composition of welding strip

, figureFileSmall=null, figureFileBig=null, tableContent=
化学元素CSiMnPSCrNiMoCu
要求值≤0.030≤1.000.5~2.5≤0.025≤0.01521.0~25.09.0~14.02.0~3.5≤0.75
实测值0.0270.381.920.0150.001 621.2513.392.590.039
), ArticleFig(id=1324796180542128407, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=CN, label=表4, caption=

焊带的化学成分

, figureFileSmall=null, figureFileBig=null, tableContent=
化学元素CSiMnPSCrNiMoCu
要求值≤0.030≤1.000.5~2.5≤0.025≤0.01521.0~25.09.0~14.02.0~3.5≤0.75
实测值0.0270.381.920.0150.001 621.2513.392.590.039
), ArticleFig(id=1324796180609237272, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=EN, label=Tab.5, caption=

The chemical composition of deposited metal of E309LT0-1 and E316LT0-1 fluxpcored wire

, figureFileSmall=null, figureFileBig=null, tableContent=
化学元素CSiMnPSCrNiMoCu
E309LT0-1要求值≤0.040≤1.000.5~2.5≤0.040≤0.03022.0~25.012.0~14.0≤0.75≤0.75
实测值0.0310.491.240.0120.002 824.3112.890.0130.000 2
E316LT0-1要求值≤0.040≤1.000.5~2.5≤0.040≤0.03017.0~20.011.0~14.02.0~3.0≤0.75
实测值0.0220.421.280.0140.003 418.3813.012.8100.043
), ArticleFig(id=1324796180680540441, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=CN, label=表5, caption=

E309LT0-1和E316LT0-1药芯焊丝熔敷金属的化学成分

, figureFileSmall=null, figureFileBig=null, tableContent=
化学元素CSiMnPSCrNiMoCu
E309LT0-1要求值≤0.040≤1.000.5~2.5≤0.040≤0.03022.0~25.012.0~14.0≤0.75≤0.75
实测值0.0310.491.240.0120.002 824.3112.890.0130.000 2
E316LT0-1要求值≤0.040≤1.000.5~2.5≤0.040≤0.03017.0~20.011.0~14.02.0~3.0≤0.75
实测值0.0220.421.280.0140.003 418.3813.012.8100.043
), ArticleFig(id=1324796180764426522, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=EN, label=Tab.6, caption=

Chemical composition of ER309L and ER316L welding wires

, figureFileSmall=null, figureFileBig=null, tableContent=
化学元素CSiMnPSCrNiMoCu
ER309L要求值≤0.030.30~0.651.00~2.50≤0.025≤0.02023.0~25.012.0~14.0≤0.75≤0.75
实测值0.0230.532.330.0140.01423.2213.940.001 00.004 9
ER316L要求值≤0.0300.30~0.651.00~2.50≤0.025≤0.02018.0~20.011.0~14.02.0~3.0≤0.75
实测值0.0190.542.040.0220.01618.8811.922.180.042
), ArticleFig(id=1324796180839923995, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=CN, label=表6, caption=

ER309L和ER316L焊丝的化学成分

, figureFileSmall=null, figureFileBig=null, tableContent=
化学元素CSiMnPSCrNiMoCu
ER309L要求值≤0.030.30~0.651.00~2.50≤0.025≤0.02023.0~25.012.0~14.0≤0.75≤0.75
实测值0.0230.532.330.0140.01423.2213.940.001 00.004 9
ER316L要求值≤0.0300.30~0.651.00~2.50≤0.025≤0.02018.0~20.011.0~14.02.0~3.0≤0.75
实测值0.0190.542.040.0220.01618.8811.922.180.042
), ArticleFig(id=1324796180919615772, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=EN, label=Tab.7, caption=

Chemical composition of the cladding layer

, figureFileSmall=null, figureFileBig=null, tableContent=
化学元素CMnSiPSNiCrMoCuN
要求值≤0.040≤2.50≤1.00≤0.030≤0.02011.0~15.016.0~20.02.0~3.0≤0.75实测
ESW试样10.0261.350.490.0160.00512.7019.672.530.040.05
试样20.0261.360.520.0160.00212.6219.572.530.040.05
FCAW试样10.0271.250.470.0160.00612.9318.222.560.010.02
试样20.0271.230.460.0150.00612.8918.082.520.010.02
GTAW试样10.0131.990.520.0210.01311.8618.492.150.010.03
试样20.0122.000.530.0210.01311.8418.422.150.010.03
), ArticleFig(id=1324796180982530333, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, language=CN, label=表7, caption=

堆焊层化学成分

, figureFileSmall=null, figureFileBig=null, tableContent=
化学元素CMnSiPSNiCrMoCuN
要求值≤0.040≤2.50≤1.00≤0.030≤0.02011.0~15.016.0~20.02.0~3.0≤0.75实测
ESW试样10.0261.350.490.0160.00512.7019.672.530.040.05
试样20.0261.360.520.0160.00212.6219.572.530.040.05
FCAW试样10.0271.250.470.0160.00612.9318.222.560.010.02
试样20.0271.230.460.0150.00612.8918.082.520.010.02
GTAW试样10.0131.990.520.0210.01311.8618.492.150.010.03
试样20.0122.000.530.0210.01311.8418.422.150.010.03
)], attaches=null, journal=Journal(id=1319354845020389520, delFlag=0, nameCn=压力容器, nameEn=Pressure Vessel Technology, nameHistory1=null, nameHistory2=null, issn=1001-4837, eissn=null, cn=34-1058/TH, coden=null, periodic=0, language=CN, oaType=null, ccby=null, superviseOffice=null, ownerOffice=null, pubOffice=null, editorOffice=null, officeType=null, aims=null, clcCode=null, officeProv=null, officeCity=null, officeAddr=null, officeZip=null, officeEmail=null, officePhone=null, editDirector=null, officeDirector=null, officeDirectorPhone=null, officeStaffNum=null, officeEmpNum=null, coverPicUrl=jxjNdnQvHSQ8b9q0zS7Bgw==, journalPrice=null, startedYear=null, abbrevIsoEn=Pressure Vessel Technology, journalRemark=null, publicationField=null, createdTime=1792488307482, updatedTime=1792488496537, createdBy=18614031015, updatedBy=13701087609, firstLetterCn=Y, firstLetterEn=Y, subjectCode=Engineering, subjectName=null, subjectCodeEn=Engineering, subjectNameEn=null, picCn=jxjNdnQvHSQ8b9q0zS7Bgw==, picEn=4fVBwqRFt4uCO8g42aXObg==, jcr=null, cjcr=null, exts=[JournalExt(id=1319355638048740090, language=CN, name=压力容器, nameHistory1=null, nameHistory2=null, managedBy=, sponsoredBy=, publishedBy=, editorOffice=, officeProv=null, officeCity=null, officeAddr=, officeZip=, editDirector=, officeDirector=null, officePhone=null, coverPicUrl=null, journalRemark=, submitArticleUrl=null, websiteUrl=, createdTime=1792488496553, updatedTime=1792488496553, createdBy=13701087609, updatedBy=13701087609, submissionGuidelinesUrl=, submissionAuthorUrl=https://ylrq.portal.founderss.cn, submissionEditorUrl=https://journal.ids.fzyun.cn, submissionReviewUrl=https://ylrq.portal.founderss.cn, submissionCeEditorUrl=, submissionAeEditorUrl=, option={"copyright":""}), JournalExt(id=1319355638103266043, language=EN, name=Pressure Vessel Technology, nameHistory1=null, nameHistory2=null, managedBy=, sponsoredBy=, publishedBy=, editorOffice=, officeProv=null, officeCity=null, officeAddr=, officeZip=, editDirector=, officeDirector=null, officePhone=null, coverPicUrl=null, journalRemark=, submitArticleUrl=null, websiteUrl=, createdTime=1792488496566, updatedTime=1792488496566, createdBy=13701087609, updatedBy=13701087609, submissionGuidelinesUrl=, submissionAuthorUrl=https://ylrq.portal.founderss.cn, submissionEditorUrl=https://journal.ids.fzyun.cn, submissionReviewUrl=https://ylrq.portal.founderss.cn, submissionCeEditorUrl=, submissionAeEditorUrl=, option={"copyright":""})], databaseList=null, tenantJournalId=1319355204128309394, websiteList=[Website(id=1319376331645764504, webName=null, webTitle=null, webDomain=null, webCopyrigh=null, webIpcNo=null, seoTitle=null, seoKeywords=null, seoDescription=null, tenantJournalId=null, journalId=1319355204128309394, journalNameCn=null, journalNameEn=null, grayFlag=null, tenantId=1146029695717560320, platformId=null, journalGroupId=null, journalGroupNameCn=null, journalGroupNameEn=null, type=1, domain=https://castjournals.cast.org.cn/joweb/ylrq/CN, language=CN, createTime=1792493430291, createBy=18614031015, updateTime=1792493471510, updateBy=18614031015, name=压力容器-中文, tplId=1146099689490845704, title=压力容器, delFlag=0, indexPage=/home, props=[WebsiteProps(id=1319376610952856568, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=articleTextType, value=kx, createTime=1792493496883, updateTime=1792493496883, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610923496437, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=banner, value=null, createTime=1792493496876, updateTime=1792493496876, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610969633787, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=grayFlag, value=0, createTime=1792493496887, updateTime=1792493496887, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610910913524, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=logo, value=https://castjournals.cast.org.cn/joweb/ylrq/CN/file/pic?fileId=jTQ3ULyAlxRu0s8fI4nfng==, createTime=1792493496873, updateTime=1792493496873, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610986411005, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=minRunFlag, value=0, createTime=1792493496891, updateTime=1792493496891, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610944467959, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=picServerUrl, value=https://castjournals.cast.org.cn/joweb/ylrq/CN/file/pic, createTime=1792493496881, updateTime=1792493496881, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610978022396, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=silenceFlag, value=0, createTime=1792493496889, updateTime=1792493496889, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610936079350, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=staticResourcePath, value=https://castjournals.cast.org.cn/joweb/cast_kjdb_cn_619/, createTime=1792493496879, updateTime=1792493496879, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610957050873, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=themeColor, value=null, createTime=1792493496884, updateTime=1792493496884, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610965439482, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=themeStyle, value=null, createTime=1792493496886, updateTime=1792493496886, creator=18614031015, updator=18614031015)]), Website(id=1319376331893228450, webName=null, webTitle=null, webDomain=null, webCopyrigh=null, webIpcNo=null, seoTitle=null, seoKeywords=null, seoDescription=null, tenantJournalId=null, journalId=1319355204128309394, journalNameCn=null, journalNameEn=null, grayFlag=null, tenantId=1146029695717560320, platformId=null, journalGroupId=null, journalGroupNameCn=null, journalGroupNameEn=null, type=1, domain=https://castjournals.cast.org.cn/joweb/ylrq/EN, language=EN, createTime=1792493430350, createBy=18614031015, updateTime=1792493467616, updateBy=18614031015, name=压力容器-英文, tplId=1146101810881728533, title=Pressure Vessel Technology, delFlag=0, indexPage=/home, props=[WebsiteProps(id=1319376586462315499, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=articleTextType, value=kx, createTime=1792493491044, updateTime=1792493491044, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586432955368, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=banner, value=null, createTime=1792493491037, updateTime=1792493491037, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586500064238, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=grayFlag, value=0, createTime=1792493491053, updateTime=1792493491053, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586420372455, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=logo, value=https://castjournals.cast.org.cn/joweb/ylrq/EN/file/pic?fileId=jTQ3ULyAlxRu0s8fI4nfng==, createTime=1792493491034, updateTime=1792493491034, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586521035760, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=minRunFlag, value=0, createTime=1792493491058, updateTime=1792493491058, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586453926890, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=picServerUrl, value=https://castjournals.cast.org.cn/joweb/ylrq/EN/file/pic, createTime=1792493491042, updateTime=1792493491042, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586512647151, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=silenceFlag, value=0, createTime=1792493491056, updateTime=1792493491056, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586441343977, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=staticResourcePath, value=https://castjournals.cast.org.cn/joweb/cast_kjdb_en_623/, createTime=1792493491039, updateTime=1792493491039, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586474898412, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=themeColor, value=null, createTime=1792493491047, updateTime=1792493491047, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586487481325, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=themeStyle, value=null, createTime=1792493491050, updateTime=1792493491050, creator=18614031015, updator=18614031015)])], journalTitle=压力容器, weixinUrl=null, journalUrl=https://www.pvtjournal.com/, iacademicId=null, status=1, seqNo=null, journalTitleEn=Pressure Vessel Technology, journalPhotoCn=jxjNdnQvHSQ8b9q0zS7Bgw==, journalPhotoEn=4fVBwqRFt4uCO8g42aXObg==, journalFirstLetter=Y, journalRecommend=null, journalNew=null, journalCollection=null, jcrJf=null, cjcrJf=null, jcrJfStr=null, cjcrJfStr=null, submissionFirstDecision=null, sciSubjectClassification=null, casSubjectClassification=null, citeScore=null, totalCitationFrequency=null, icpCode=null, psCode=null, advertisingLicenseCode=null, copyrightInformation=null, country=null, option=, provinceCode=null, provinceName=null, collectFlag=false, interPubPlatform=, interPubPlatformUrl=null), detailUrlCn=https://castjournals.cast.org.cn/joweb/ylrq/CN/10.3969/j.issn.1001-4837.2025.06.003, detailUrlEn=https://castjournals.cast.org.cn/joweb/ylrq/EN/10.3969/j.issn.1001-4837.2025.06.003, pdfUrlCn=https://castjournals.cast.org.cn/joweb/ylrq/CN/PDF/10.3969/j.issn.1001-4837.2025.06.003, pdfUrlEn=https://castjournals.cast.org.cn/joweb/ylrq/EN/PDF/10.3969/j.issn.1001-4837.2025.06.003, aliStartDate=0, aliEndDate=0, collectionFlag=false, citedCount=null, citedUrl=null, previewStatus=0, delFlag=0, hasFullText=1, orderTime=1751212800000, fullTextJson=null, articleText=null, reference=null)
收藏切换
20MnNiMo钢表面TP316L不锈钢堆焊工艺研究及应用
王雪骄
压力容器 | 试验研究 2025,42(6): 19-24
收起
收藏切换
压力容器 |试验研究 2025 , 42 (6) : 19 -24
20MnNiMo钢表面TP316L不锈钢堆焊工艺研究及应用
全屏
[Author(id=1324796178667274492, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, orderNo=0, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=NN791H528@163.com, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1324796178738577662, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, authorId=1324796178667274492, language=EN, stringName=Xuejiao WANG, firstName=Xuejiao, middleName=null, lastName=WANG, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1324796178826658047, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, authorId=1324796178667274492, language=CN, stringName=王雪骄, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=null, address=1二重(德阳)重型装备有限公司,四川 德阳 618000, bio={"content":"

王雪骄(1978),女,正高级工程师,主要从事压力容器焊接制造技术的研究与开发工作,通信地址:618000四川省德阳市二重(德阳)重型装备有限公司重型压力容器及核电技术研究所,E-mail:。

"}, bioImg=null, bioContent=

王雪骄(1978),女,正高级工程师,主要从事压力容器焊接制造技术的研究与开发工作,通信地址:618000四川省德阳市二重(德阳)重型装备有限公司重型压力容器及核电技术研究所,E-mail:。

, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1324796178545639672, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, xref=1, ext=[AuthorCompanyExt(id=1324796178554028281, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, companyId=1324796178545639672, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China), AuthorCompanyExt(id=1324796178566611194, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324796175555100911, companyId=1324796178545639672, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1二重(德阳)重型装备有限公司,四川 德阳 618000)])])]
王雪骄
作者信息
  • 1二重(德阳)重型装备有限公司,四川 德阳 618000
作者简介:

王雪骄(1978),女,正高级工程师,主要从事压力容器焊接制造技术的研究与开发工作,通信地址:618000四川省德阳市二重(德阳)重型装备有限公司重型压力容器及核电技术研究所,E-mail:。

Research and application of TP316L stainless steel cladding process on 20MnNiMo steel surface
Xuejiao WANG
Affiliations
  • 1Erzhong(Deyang) Heavy Equipment Co.,Ltd.,Deyang 618000,China
出版时间: 2025-06-30 doi: 10.3969/j.issn.1001-4837.2025.06.003
文章导航
收藏切换

针对20MnNiMo钢在特定环境下的耐腐蚀性能不足问题,采用电渣焊(ESW)、药芯焊丝电弧焊(FCAW)和钨极气体保护焊(GTAW) 3种工艺,在其表面堆焊TP316L不锈钢层以提高其耐蚀性。通过焊接工艺试验确定了稳定的焊接参数,并对堆焊层进行了化学成分分析、侧弯试验、硬度测试、晶间腐蚀试验及金相组织观察。结果表明,堆焊层化学成分均匀,且符合标准要求(Ni的质量分数为11.0%~15.0%,Cr的质量分数为16.0%~20.0%);侧弯试验无裂纹产生;硬度值均低于250HV10;晶间腐蚀性能合格;显微组织为均匀的奥氏体基体+少量铁素体。研究证实,ESW,FCAW和GTAW 3种工艺均能满足设备制造要求,ESW采用单层带极堆焊,堆焊层厚度4.0~4.5 mm;FCAW和GTAW堆焊时需采用过渡层TP309L+耐蚀层TP316L双层堆焊,耐蚀层FCAW至少1层,耐蚀层GTAW至少2层,堆焊层总厚度5.0~5.5 mm。该研究为20MnNiMo钢在腐蚀环境中的工程应用提供了可靠的数据支撑和工艺指导,具有重要的工程实践价值。

20MnNiMo钢  /  TP316L钢  /  电渣焊  /  药芯焊丝电弧焊  /  钨极气体保护焊

To address the insufficient corrosion resistance of 20MnNiMo steel in specific environments,three welding processes,electroslag welding (ESW),flux cored arc welding (FCAW),and gas tungsten arc welding (GTAW),were employed to overlay a TP316L stainless steel layer on its surface to improve corrosion resistance.Stable welding parameters were determined through welding process tests,and the cladding layers were subjected to chemical composition analysis,side bend tests,hardness tests,intergranular corrosion tests,and metallographic structure observation.The results indicate that the chemical composition of the cladding layers is uniform and meets standard requirements(Ni mass fraction:11.0% to 15.0%,Cr mass fraction:16.0% to 20.0%);no cracks were generated in the side bend tests;hardness values were all below 250HV10;intergranular corrosion performance was qualified;and the microstructure consisted of a uniform austenitic matrix with a small amount of ferrite.The study confirms that all three processes,ESW,FCAW,and GTAW,can meet equipment manufacturing requirements.ESW uses single layer strip cladding with a cladding thickness of 4.0 to 4.5 mm;FCAW and GTAW require a two layer cladding of transition layer TP309L and corrosion resistant layer TP316L,with at least one layer for FCAW and at least two layers for GTAW in the corrosion resistant layer,and a total cladding thickness of 5.0 to 5.5 mm.This research provides reliable data support and process guidance for the engineering application of 20MnNiMo steel in corrosive environments,demonstrating significant practical engineering value.

20MnNiMo steel  /  TP316L steel  /  electroslag welding  /  flux cored arc welding  /  gas tungsten arc welding
王雪骄. 20MnNiMo钢表面TP316L不锈钢堆焊工艺研究及应用. 压力容器, 2025 , 42 (6) : 19 -24 . DOI: 10.3969/j.issn.1001-4837.2025.06.003
Xuejiao WANG. Research and application of TP316L stainless steel cladding process on 20MnNiMo steel surface[J]. Pressure Vessel Technology, 2025 , 42 (6) : 19 -24 . DOI: 10.3969/j.issn.1001-4837.2025.06.003
20MnNiMo钢作为一种高强度、高韧性的合金钢,具有优良的高温强度、抗疲劳强度、抗低温冲击性能[1],广泛应用于石油、化工、海洋等领域压力容器的制造。但在特定环境下其耐腐蚀性相对较差,易发生腐蚀现象,影响了其使用寿命和安全性。而堆焊作为一种有效的表面改性技术,可以通过在母材表面堆焊一层耐腐蚀、耐磨损的材料来提高其综合性能。目前,对于20MnNiMo钢的焊接及相关性能的研究较多[1-5],但对于20MnNiMo钢表面的堆焊研究很少。文中研究试验依托某海洋项目设备开展工作,旨在对20MnNiMo钢表面TP316L不锈钢堆焊工艺进行研究,以期获得满足设备制造要求的堆焊层。
该海洋项目设备壳体材料为20MnNiMo钢锻件,所有与介质接触的壳体内表面应堆焊厚度不小于4 mm的TP316L不锈钢堆焊层,堆焊层表面下1.5~2 mm范围内的化学成分应满足表1中要求。
模拟设备制造的最大焊后热处理(Max.PWHT)为(590±10) ℃×90+1 h,最小焊后热处理(Min.PWHT)为(590±10) ℃×30+1 h。在模拟Min.PWHT和Max.PWHT状态下进行硬度试验;在Max.PWHT状态下进行弯曲、晶间腐蚀、微观金相试验。
在满足制造技术要求的前提条件下,结合依托设备结构,尽可能选用堆焊效率高的焊接方法。因此,对于大面积堆焊部位,采用堆焊效率高的电渣焊(ESW)带极堆焊;对于局部焊带不能堆焊的部位及补堆部位,采用焊接效率较高的药芯焊丝电弧焊(FCAW)堆焊;对于小孔内壁,采用钨极气体保护焊(GTAW)堆焊。
试件采用20MnNiMo钢锻件加工制备,试件材料的化学成分见表2。试件材料模拟Max.PWHT和Min.PWHT后的力学性能见表3。
综合考虑焊接工艺评定试件厚度覆盖和堆焊时试件变形问题,试件的规格:ESW为50 mm×250 mm×400 mm,FCAW为40 mm×250 mm×400 mm,GTAW为5 mm×250 mm×400 mm。
20MnNiMo钢表面堆焊TP316L不锈钢属于异种金属的焊接,堆焊层熔敷金属的稀释和堆焊层熔合区的塑性对堆焊层的质量至关重要[6]。由于带极堆焊中电渣焊(ESW)与埋弧焊(SAW)相比,具有熔敷效率高、熔深浅且均匀、成形好,表面质量优良、焊剂消耗低等优点[7-8],故带极堆焊方法选择单层带极ESW堆焊。选择国内某公司的焊材:焊带为EQ309LMo(60 mm×0.5 mm)和配套焊剂,焊带的化学成分如表4所示。
FCAW和GTAW堆焊时,考虑堆焊过程中合金元素的烧损和稀释,为满足整个堆焊层有效厚度的要求,采用双层堆焊:第1层为过渡层,选用Cr,Ni合金元素含量更高的TP309L焊材进行过渡;第2层为耐蚀层,采用与制造要求一致的TP316L焊材进行堆焊。
选择国内某公司的焊材,FCAW:过渡层药芯焊丝E309LT0-1,⌀1.6 mm,耐蚀层药芯焊丝E316LT0-1,⌀1.6 mm,熔敷金属化学成分如表5所示;GTAW:过渡层焊丝ER309L,⌀1.2 mm,耐蚀层焊丝ER316L,⌀1.2 mm,焊丝的化学成分如表6所示。
根据表2可以看出,20MnNiMo钢的碳当量较高,具有较大的淬硬倾向和氢致裂纹敏感性,因此在焊接过程中,需要特别注意防止裂纹的产生。可通过采用预热、控制焊接参数等方法来解决这些问题。较低的预热及层间温度有利于减弱不锈钢堆焊层δ相→σ脆性相的转变倾向,防止晶间腐蚀发生[9],结合20MnNiMo钢焊接时的预热温度和以往堆焊制造经验,单层堆焊和双层堆焊中,过渡层的堆焊预热温度≥125 ℃。为避免因堆焊层温度过高而引起熔敷金属晶粒粗大、不锈钢敏化及易产生热裂纹等问题,焊接过程中,过渡层层间温度控制在125~200 ℃,耐蚀层层间温度<100 ℃。
根据文献[10],单层电渣堆焊层厚度在4.5~5.0 mm时,堆焊表面以下3 mm 范围内堆焊层化学成分比较均匀。因此,ESW堆焊1层,堆焊层总厚度按照4.0~4.5 mm控制。鉴于技术要求中堆焊层化学成分取样位置在表面下1.5~2.0 mm处,而FCAW一层的堆焊厚度约2.5 mm,同时,考虑堆焊成分稀释的问题,将FCAW工艺设置为堆焊2层:TP309L过渡层1层+TP316L耐蚀层1层,过渡层堆焊厚度为2.0~2.5 mm,耐蚀层堆焊厚度为2.5~3.0 mm,堆焊层总厚度按照5.0~5.5 mm控制,采用99.5%的CO2气体保护焊接。对于GTAW,一层的堆焊厚度不能达到2.5 mm以上,为保证堆焊层总厚度和堆焊层的有效厚度,将GTAW工艺设置为堆焊3层:TP309L过渡层1层+TP316L耐蚀层2层,每层堆焊厚度为1.5~2.0 mm,堆焊层总厚度按照5.0~5.5 mm控制,采用99.99%的氩气保护焊接。通过焊接试验对工艺参数进行调整和优化,筛选出焊接过程稳定性、焊缝成形美观、焊接工艺性好的规范参数,结合设备制造技术条件和NB/T 47014—2011《承压设备焊接工艺评定》中的相关要求,进行焊接工艺评定试验。
从焊态表面测量堆焊层最小厚度:ESW为4.0 mm,满足堆焊层总厚度4.0~4.5 mm的要求;FCAW为5.1 mm,GTAW为5.2 mm,均满足设备制造技术要求中堆焊层总厚度5.0~5.5 mm的要求。
焊态下,在堆焊层表面下1.5~2.0 mm范围内取样进行化学成分分析,每种焊接方法取样2处,化学成分检测结果见表7。可以看出,3种焊接方法的堆焊层化学成分均满足技术条件中的要求,且成分适中,不同位置波动小。
试件模拟Max.PWHT和Min.PWHT后进行性能检测。
(1)剖面检查(Max.PWHT热处理状态)。
在堆焊试件上的焊道搭接处取剖面,经酸洗后用5倍放大镜观察,焊缝搭接处未发现肉眼可见的焊接缺陷。
(2)弯曲试验(Max.PWHT热处理状态)。
采用横向大侧弯2件(试样长轴垂直于堆焊方向)、纵向大侧弯2件(试样长轴平行于堆焊方向),试样尺寸见图1(a);采用横向小侧弯2件(试样长轴垂直于堆焊方向)、纵向小侧弯2件(试样长轴平行于堆焊方向),试样尺寸见图1(b)[11]。按照弯曲试验要求(D=4a,α=180°),弯曲试验后在堆焊层和熔合线上均没有裂纹和未融合缺陷,说明堆焊层结合面具有良好的塑性。
(3)晶间腐蚀试验(Max.PWHT热处理状态)。
将堆焊层表面磨平,向下取厚度2 mm试样进行晶间腐蚀试验,试样尺寸80 mm×20 mm×2 mm,共2件。按照GB/T 4334—2020《金属和合金的腐蚀 奥氏体及铁素体-奥氏体(双相)不锈钢晶间腐蚀试验方法》中方法E进行不锈钢硫酸-硫酸铜抗晶间腐蚀试验。所有试样经弯曲180°后,在10倍放大镜下观察弯曲试样的外表面,均未发现因晶间腐蚀而产生的裂纹。
(4)硬度测量(Min.PWHT和Max.PWHT热处理状态)。
按GB/T 4340.1—2009《金属材料 维氏硬度试验 第1部分:试验方法》的要求,在堆焊试件的横截面上取样,硬度测试包括熔合线和热影响区,每区测量3处,每处测试5点。3种焊接方法在Min.PWHT和Max.PWHT状态下的检测结果见图2,硬度值均小于250HV10。3种方法的堆焊试件横截面熔合线和热影响区硬度测量值差距不大。
(5)微观金相组织分析(Max.PWHT热处理状态)。
在堆焊层表面及以下2.0 mm深度位置取样进行微观金相组织分析,其结果见图3。金相组织为均匀的奥氏体+少量铁素体双向组织。满足技术条件要求:堆焊层表面及以下2 mm深度以内金相组织为均匀的奥氏体+铁素体双向组织。
对比3种焊接方法,ESW晶粒相对粗大,柱状晶发达;FCAW晶粒较细小,呈等轴晶或树枝晶形态;GTAW晶粒最为细小,呈细小等轴晶或胞状晶形态。这是由于焊接热输入及熔池保护方式的不同,致使熔池冷却速度和晶粒生长条件不同而造成的。ESW热输入最高,熔池冷却速度慢,晶粒有足够时间生长,形成较为粗大的柱状晶组织;FCAW次之,药芯焊丝中的造气剂和造渣剂形成保护气氛,电弧稳定性较好,熔池冷却速度相对较快,抑制了晶粒的过度生长,晶粒较为细小;GTAW最低,电弧集中,熔池冷却速度快,晶粒来不及长大即被“冻结”。
综合上述检验结果可以看出,试验采用的堆焊工艺能获得化学成分和性能均满足设备制造要求的堆焊层,也验证了堆焊工艺的正确性,具备在产品上应用的条件。
经过前期的焊接工艺性试验,在合格的堆焊工艺评定支撑下,将上述堆焊工艺在产品内壁进行堆焊应用。结果表明,产品堆焊层成型情况良好,表面平整。产品堆焊厚度:ESW为4.3~5.0 mm;FCAW为5.3~5.6 mm;GTAW为5.2~5.3 mm。在产品堆焊层表面下1.5~2.0 mm范围内取样进行化学成分检测,各元素值均满足制造技术条件要求,且堆焊层经100%PT和100%UT检测,均满足Ⅰ级合格要求,应用效果良好。
(1)在20MnNiMo钢上堆焊不锈钢时的单层及过渡层时预热温度≥125 ℃,层间温度控制为125~200 ℃。
(2)ESW,FCAW和GTAW 3种焊接方法在20MnNiMo钢试件上堆焊后,堆焊层成型情况良好,表面平整,化学成分、力学性能和耐腐蚀性能均满足设备制造要求。其中,单层带极ESW堆焊层厚度4.0~4.5 mm;焊丝堆焊时需采用过渡层TP309L+耐蚀层TP316L双层堆焊,耐蚀层FCAW至少1层,耐蚀层GTAW至少2层,堆焊层总厚度满足5.0~5.5 mm要求。
(3)通过对20MnNiMo钢表面TP316L不锈钢堆焊工艺研究及成功应用案例,为该材料的工程应用提供了数据支持和实践指导。

参考文献 引证文献
排序方式:
1
王强,麻永林,陈重毅,等.焊接热输入对厚壁20MnNiMo钢焊缝性能的影响[J].山西冶金,2016,39(6):1-4.
WANG Q,MA Y L,CHEN Z Y,et al.Effect of welding heat input on properties of weld seam of thick 20MnNiMo steel[J].Shanxi Metallurgy,2016,39(6):1-4.
2
陈重毅,麻永林,邢淑清,等.焊接热输入对特厚板20MnNiMo焊接残余应力的影响[J].材料热处理学报,2013,34(1):76-80.
CHEN Z Y,MA Y L,XING S Q,et al.Effect of welding heat input on welding residual stress in submerged‑arc welds of thick plate 20MnNiMo joints[J].Transactions of Materials and Heat Treatment,2013,34(1):76-80.
3
迟露鑫,陈重毅,麻永林,等.焊后热处理对特厚板 20MnNiMo焊接残余应力的影响[J].材料热处理学报,2012,33(4):96-99.
CHI L X,CHEN Z Y,MA Y L,et al.Effect of post‑weld heat treatment on residual stress in submerged‑arc welds of 20MnNiMo steel heavy plate [J].Transactions of Materials and Heat Treatment,2012,33(4):96-99.
4
张显辉,焦伟,谭长瑛.20MnNiMo钢焊接热影响区的组织和韧性及其氢致裂纹特征[J].焊接学报,2000,21(1):9-12.
ZHANG X H,JIAO W,TAN C Y.HAZ structure,toughness and characteristics to hydrogen‑induced cracking(HIC) of steel 20MnNiMo[J].Transactions of the China Welding Institution,2000,21(1):9-12.
5
张显辉,焦伟,谭长瑛.20MnNiMo钢焊接氢致裂纹特征(Ⅱ)[J].焊接学报,2002,23(3):23-25.
ZHANG X H,JIAO W,TAN C Y.Hydrogen‑induced cracking feature of steel 20MnNiMo(Ⅱ)[J].Transactions of the China Welding Institution,2002,23(3):23-25.
6
刘玉华.CO2药芯焊丝气保焊(FCAW)在加氢反应器接管内壁不锈钢堆焊中的应用[J].金属加工(热加工),2009(12):25-29.
LIU Y H.Application of CO2 flux‑cored wire arc welding (FCAW) in stainless steel surfacing on the inner wall of hydrogenation reactor nozzle[J].MW Metal Forming,2009(12):25-29.
7
王晖球,王雪骄,叶小松.国产不锈钢双电渣堆焊材料在加钒钢加氢反应器上的应用[J].大型铸锻件,2021(5):28-31.
WANG H Q,WANG X J,YE X S.Application of domestic stainless steel double‑layer electro‑slag surfacing on the vanadium steel hydrogenation reactor[J].Heavy Casting and Forging,2021(5):28-31.
8
邢卓.管板带极电渣堆焊双相不锈钢工艺[J].压力容器,2024,41(11):74-84.
XING Z.Overview of surfacing duplex stainless steel on tubesheets by electroslag strip welding[J].Pressure Vessel Technology,2024,41(11):74-84.
9
陈志林,刘应虎.90 mm宽带极堆焊奥氏体不锈钢的化学成分及铁素体FN分析[J].压力容器,2011,28(11):41-46.
CHEN Z L,LIU Y H.Chemical elements and ferrite number analysis of austenitic stainless steel surfacing process with 90 mm strip electrode[J].Pressure Vessel Technology,2011,28(11):41-46.
10
王雪骄,范阳阳,晏君文,等.2.25Cr-1Mo-0.25V钢上国产焊材单层带极电渣堆焊工艺研究[J].大型铸锻件,2023(5):32-36.
WANG X J,FAN Y Y,YAN J W,et al.The technology study of single‑layer ESW cladding on 2.25Cr-1Mo-0.25V steel surface using domestic welding materials[J].Heavy Casting and Forging,2023(5):32-36.
11
王雪骄,王迎君,晏君文,等.加氢反应器E309L过渡层经PWHT后堆焊或焊接E347对基体材料的影响[J].压力容器,2016,33(3):61-68.
WANG X J,WANG Y J,YAN J W,et al.Influence of welding or cladding E347 on E309L transition layer after PWHT to substrate material in hydrogenation reactor[J].Pressure Vessel Technology,2016,33(3):61-68.
2025年第42卷第6期
218
93
0
引用本文
BibTeX
文章信息
doi: 10.3969/j.issn.1001-4837.2025.06.003
  • 接收时间:2025-01-02
  • 首发时间:2026-11-04
  • 出版时间:2025-06-30
补充材料
相关文章
文章信息
作者
出版历史
  • 收稿日期:2025-01-02
  • 修回日期:2025-04-23
基金
作者信息
    1二重(德阳)重型装备有限公司,四川 德阳 618000
参考文献
分享链接
https://castjournals.cast.org.cn/joweb/ylrq/CN/10.3969/j.issn.1001-4837.2025.06.003
分享至
全文二维码

扫描看全文

引用本文
BibTeX
本文的引用情况
2种不同金属材料的力学参数
科
Family
属数
Number of
genus
种数
Number of
species
占总种数比例
Percentage of
total species (%)
属
Genus
种数
Number of
species
占总种数比例
Percentage of total
species (%)
鹅膏菌科Amanitaceae 2 11 5.26 鹅膏菌属 Amanita 10 4.78
小菇科 Mycenaceae 2 12 5.74 丝盖伞属 Inocybe 5 2.39
多孔菌科 Polyporaceae 8 14 6.70 蜡蘑属 Laccaria 5 2.39
红菇科 Russulaceae 3 23 11.00 小皮伞属 Marasmius 6 2.87
小菇属 Mycena 11 5.26
光柄菇属 Pluteus 5 2.39
红菇属 Russula 17 8.13
栓菌属 Trametes 5 2.39
关闭全屏