Article(id=1324788948941283499, tenantId=1146029695717560320, journalId=1319355204128309394, issueId=1324788931312628309, articleNumber=null, orderNo=null, doi=10.3969/j.issn.1001-4837.2025.03.009, pmid=null, cstr=null, oa=null, hot=null, price=null, onlineType=0, articleFormat=0, articleType=null, articleTypeStr=null, receivedDate=1737216000000, receivedDateStr=2025-01-19, revisedDate=1740672000000, revisedDateStr=2025-02-28, acceptedDate=null, acceptedDateStr=null, onlineDate=1793783898816, onlineDateStr=2026-11-04, pubDate=1743264000000, pubDateStr=2025-03-30, doiRegisterDate=null, doiRegisterDateStr=null, onlineIssueDate=1793783898816, onlineIssueDateStr=2026-11-04, onlineJustAcceptDate=null, onlineJustAcceptDateStr=null, onlineFirstDate=null, onlineFirstDateStr=null, sourceXml=null, magXml=null, createTime=1793783898816, creator=13701087609, updateTime=1793783898816, updator=13701087609, issue=Issue{id=1324788931312628309, tenantId=1146029695717560320, journalId=1319355204128309394, year='2025', volume='42', issue='3', pageStart='1', pageEnd='86', issueExtLink='null', onlineDate='null', pubDate='1743264000000', pubDateStr='2025-03-30', beforeIssueId=null, nextIssueId=null, price=null, status=1, issueComplete=1, articleOrder=1, issueType=-1, specialIssue=null, createTime=1793783894613, creator='13701087609', updateTime=1793787513690, updator='13701087609', preIssue=null, nextIssue=null, articleTotal=null, ext={EN=IssueExt(id=1324804110888874893, tenantId=1146029695717560320, journalId=1319355204128309394, issueId=1324788931312628309, language=EN, specialIssueTitle=, coverIllustrator=null, specialIssueEditor=, specialIssueAbout=), CN=IssueExt(id=1324804110888874894, tenantId=1146029695717560320, journalId=1319355204128309394, issueId=1324788931312628309, language=CN, specialIssueTitle=, coverIllustrator=null, specialIssueEditor=, specialIssueAbout=)}, issueFiles=null, downloadFileDto=null}, startPage=71, endPage=78, ext={EN=ArticleExt(id=1324788949213913261, articleId=1324788948941283499, tenantId=1146029695717560320, journalId=1319355204128309394, language=EN, title=Analysis of corrosion and leakage causes in heat exchangers of low‑temperature methanol washing units, columnId=1324788949125832876, journalTitle=Pressure Vessel Technology, columnName=Safety Analyses, runingTitle=null, highlight=null, articleAbstract=

To analyze the corrosion and leakage causes in heat exchangers of low‑temperature methanol washing unit,scanning electron microscopy (SEM),energy‑dispersive spectroscopy (EDS) and X‑ray diffraction (XRD) were used to examine the microstructure,elemental distribution,and phase composition of the failed tubes.X‑ray fluorescence (XRF) was employed to determine the elemental content of sludge in the header.Additionally,corrosion simulation experiments were conducted to characterize the corrosive effects of sulfur‑rich methanol on the heat exchanger material.Results showed that multiple corrosion perforations (maximum diameter:2.5 mm) existed in the failed tubes,with perforation walls nearly perpendicular and no abnormal thinning observed in surrounding areas.The corrosion products primarily consisted of iron‑sulfur compounds,and significant sulfur‑containing components were detected in the sludge.High temperature markedly accelerated material corrosion,with a corrosion rate reaching 0.138 mm/a at 80 ℃.During operation,partial desorption of H2S from sulfur‑rich methanol formed an H2S-H2O electrochemical corrosion environment,leading to uniform thinning of the tubes.Under‑deposit corrosion caused by sludge adhesion was identified as the primary cause of perforation.Measures such as adding corrosion and scale inhibitors and upgrading the heat exchanger material can mitigate corrosion risks and extend equipment service life.The research can provide theoretical basis and engineering reference for corrosion prevention and control of low‑temperature methanol washing unit and heat exchanger selection.

, authors=Guoqing SU1, Yan LI1, Jianwen ZHANG1, Zhijun ZHANG2, authorsList=Guoqing SU, Yan LI, Jianwen ZHANG, Zhijun ZHANG, authorCompany=null, correspAuthors=Jianwen ZHANG, authorNote=null, correspAuthorsNote=null, copyrightStatement=null, copyrightOwner=null, extLink=null, articleAbsUrl=null, sourceXml=null, magXml=null, pdfUrl=null, pdf=null, pdfFileSize=null, pdfExtLink=null, richHtmlUrl=null, mobilePdfUrl=null, reviewReport=null, pdfFirstPage=null, abstractGraph=null, abstractGraphContent=null, abstractVideo=null, citation=null, cebUrl=null, magXmlContent=null, mapNumber=null, fund=null), CN=ArticleExt(id=1324788951214596288, articleId=1324788948941283499, tenantId=1146029695717560320, journalId=1319355204128309394, language=CN, title=低温甲醇洗装置换热器腐蚀泄漏原因分析, columnId=1320423011124097617, journalTitle=压力容器, columnName=安全分析, runingTitle=null, highlight=null, articleAbstract=

为分析低温甲醇洗装置换热器的腐蚀泄漏原因,利用扫描电镜(SEM)、能谱仪(EDS)和X射线衍射仪(XRD),分别测定了失效管束的微观结构、元素分布和物相组成;利用X射线荧光光谱仪(XRF)测定封头处污泥的元素含量。此外,通过腐蚀模拟试验表征了富硫甲醇对换热管材质的腐蚀特性。结果表明,失效换热管存在多处腐蚀穿孔,最大直径为2.5 mm,腐蚀穿孔壁面近似垂直,且在其周围区域未发现异常减薄;腐蚀产物主要为硫铁化合物,同时在污泥中检测出大量含硫成分;高温显著加剧换热管材料腐蚀,80 ℃时腐蚀速率达到0.138 mm/a;在换热器运行过程中,富硫甲醇中H2S部分解吸形成了H2S-H2O电化学腐蚀环境,导致换热管出现均匀减薄,而污泥附着引发的垢下腐蚀是换热管腐蚀穿孔的主要原因。采取添加缓蚀阻垢剂、升级换热器材质等措施,可降低换热器的腐蚀风险,延长设备的运行周期。研究结果可为低温甲醇洗装置的腐蚀防控及换热器选型提供理论依据和工程参考。

, authors=苏国庆1, 李彦1, 张建文1, 张志军2, authorsList=苏国庆, 李彦, 张建文, 张志军, authorCompany=null, correspAuthors=张建文, authorNote=

苏国庆(1994),男,主要研究方向为多相流腐蚀,通信地址:100029北京市朝阳区北三环东路15号北京化工大学机电工程学院,E-mail:。

, correspAuthorsNote=
张建文(1969),男,教授,主要研究领域为化学工程、新/非常规能源技术与装备及化工安全等,通信地址:100029 北京市朝阳区北三环东路15号北京化工大学机电工程学院,E-mail:。
, copyrightStatement=作者向本刊所投稿件一经本刊录用,则该论文的复制权、发行权、信息网络传播权、翻译权、汇编权等权利视为自动转让给本刊。本刊为国内各主要数据库收录期刊,本刊所发表的稿件将同时通过因特网进行网络出版或提供信息服务(包括印刷版、光盘版和网络版等各种使用方式)。, copyrightOwner=null, extLink=null, articleAbsUrl=null, sourceXml=cfdiIYIQ+CcyyfGvg7YS8A==, magXml=ushef6PobHFoFDc/220lww==, pdfUrl=null, pdf=Z21zCTleGyLNtMJxjHjB8w==, pdfFileSize=6782796, pdfExtLink=null, richHtmlUrl=null, mobilePdfUrl=null, reviewReport=null, pdfFirstPage=null, abstractGraph=LPaM00CoHvmh+6QOvyCMzQ==, abstractGraphContent=null, abstractVideo=null, citation=null, cebUrl=null, magXmlContent=TTbFEk+M80FlYb+PpQXAYA==, mapNumber=null, fund=null)}, authors=[Author(id=1324788953219473608, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, orderNo=0, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=1556544322@qq.com, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1324788953328525514, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, authorId=1324788953219473608, language=EN, stringName=Guoqing SU, firstName=Guoqing, middleName=null, lastName=SU, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1College of Mechanical and Electrical Engineering,Beijing University of Chemical Technology,Beijing 100029,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1324788953395634379, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, authorId=1324788953219473608, language=CN, stringName=苏国庆, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1北京化工大学 机电工程学院,北京 100029, bio={"content":"

苏国庆(1994),男,主要研究方向为多相流腐蚀,通信地址:100029北京市朝阳区北三环东路15号北京化工大学机电工程学院,E-mail:。

"}, bioImg=null, bioContent=

苏国庆(1994),男,主要研究方向为多相流腐蚀,通信地址:100029北京市朝阳区北三环东路15号北京化工大学机电工程学院,E-mail:。

, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1324788951541752001, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, xref=1, ext=[AuthorCompanyExt(id=1324788951550140610, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788951541752001, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1College of Mechanical and Electrical Engineering,Beijing University of Chemical Technology,Beijing 100029,China), AuthorCompanyExt(id=1324788951558529219, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788951541752001, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1北京化工大学 机电工程学院,北京 100029)])]), Author(id=1324788953487909069, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, orderNo=1, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1324788953571795151, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, authorId=1324788953487909069, language=EN, stringName=Yan LI, firstName=Yan, middleName=null, lastName=LI, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1College of Mechanical and Electrical Engineering,Beijing University of Chemical Technology,Beijing 100029,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1324788953638904016, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, authorId=1324788953487909069, language=CN, stringName=李彦, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1北京化工大学 机电工程学院,北京 100029, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1324788951541752001, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, xref=1, ext=[AuthorCompanyExt(id=1324788951550140610, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788951541752001, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1College of Mechanical and Electrical Engineering,Beijing University of Chemical Technology,Beijing 100029,China), AuthorCompanyExt(id=1324788951558529219, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788951541752001, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1北京化工大学 机电工程学院,北京 100029)])]), Author(id=1324788953710207186, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, orderNo=2, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=zhangjw@mail.buct.edu.cn, emailSecond=null, emailThird=null, correspondingAuthor=1, authorType=1, ext={EN=AuthorExt(id=1324788953789898964, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, authorId=1324788953710207186, language=EN, stringName=Jianwen ZHANG, firstName=Jianwen, middleName=null, lastName=ZHANG, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1College of Mechanical and Electrical Engineering,Beijing University of Chemical Technology,Beijing 100029,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1324788953873785045, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, authorId=1324788953710207186, language=CN, stringName=张建文, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1北京化工大学 机电工程学院,北京 100029, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1324788951541752001, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, xref=1, ext=[AuthorCompanyExt(id=1324788951550140610, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788951541752001, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1College of Mechanical and Electrical Engineering,Beijing University of Chemical Technology,Beijing 100029,China), AuthorCompanyExt(id=1324788951558529219, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788951541752001, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1北京化工大学 机电工程学院,北京 100029)])]), Author(id=1324788953945088215, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, orderNo=3, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1324788954008002777, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, authorId=1324788953945088215, language=EN, stringName=Zhijun ZHANG, firstName=Zhijun, middleName=null, lastName=ZHANG, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=2, address=2National Energy Group Ningxia Coal Industry Co.,Ltd.,Coal to Oil Branch,Yinchuan 750411,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1324788954075111642, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, authorId=1324788953945088215, language=CN, stringName=张志军, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=2, address=2国家能源集团 宁夏煤业有限责任公司 煤制油分公司,银川 750411, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1324788953139781828, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, xref=2, ext=[AuthorCompanyExt(id=1324788953148170437, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788953139781828, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=2National Energy Group Ningxia Coal Industry Co.,Ltd.,Coal to Oil Branch,Yinchuan 750411,China), AuthorCompanyExt(id=1324788953156559046, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788953139781828, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=2国家能源集团 宁夏煤业有限责任公司 煤制油分公司,银川 750411)])])], keywords=[Keyword(id=1324788954217717979, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=EN, orderNo=1, keyword=heat exchanger), Keyword(id=1324788954280632540, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=EN, orderNo=2, keyword=leakage), Keyword(id=1324788954356130013, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=EN, orderNo=3, keyword=corrosion analysis), Keyword(id=1324788954435821790, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=EN, orderNo=4, keyword=H2S corrosion), Keyword(id=1324788954502930655, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=EN, orderNo=5, keyword=under‑deposit corrosion), Keyword(id=1324788954574233824, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=CN, orderNo=1, keyword=换热器), Keyword(id=1324788954645536993, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=CN, orderNo=2, keyword=泄漏), Keyword(id=1324788954712645858, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=CN, orderNo=3, keyword=腐蚀分析), Keyword(id=1324788954788143331, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=CN, orderNo=4, keyword=H2S腐蚀), Keyword(id=1324788954888806628, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=CN, orderNo=5, keyword=垢下腐蚀)], refs=[Reference(id=1324788958877589760, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2022, volume=50, issue=11, pageStart=74, pageEnd=78, url=null, language=null, rfNumber=1, rfOrder=0, authorNames=赖宁, 于杰, 魏成, journalName=化学工程, refType=null, unstructuredReference=赖宁,于杰,魏成,等.低温甲醇洗装置运行问题及对策[J].化学工程,2022,50(11):74-78., articleTitle=低温甲醇洗装置运行问题及对策, refAbstract=null), Reference(id=1324788958957281537, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2022, volume=50, issue=11, pageStart=74, pageEnd=78, url=null, language=null, rfNumber=1, rfOrder=1, authorNames=LAI N, YU J, WEI C, journalName=Chemical Engineering (China), refType=null, unstructuredReference=LAI N,YU J,WEI C,et al.Problems and counter measures of rectisol plant during operation[J].Chemical Engineering (China),2022,50(11):74-78., articleTitle=Problems and counter measures of rectisol plant during operation, refAbstract=null), Reference(id=1324788959036973314, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2021, volume=null, issue=10, pageStart=181, pageEnd=185, url=null, language=null, rfNumber=2, rfOrder=2, authorNames=王伟, 杜丽, journalName=化学工程与装备, refType=null, unstructuredReference=王伟,杜丽.低温甲醇洗装置贫甲醇换热器换热管失效分析[J].化学工程与装备,2021(10):181-185., articleTitle=低温甲醇洗装置贫甲醇换热器换热管失效分析, refAbstract=null), Reference(id=1324788959120859395, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2021, volume=null, issue=10, pageStart=181, pageEnd=185, url=null, language=null, rfNumber=2, rfOrder=3, authorNames=WANG W, DU L, journalName=Chemical Engineering & Equipment, refType=null, unstructuredReference=WANG W,DU L.Failure analysis of lean methanol heat exchanger tube in the low‑temperature methanol wash unit[J].Chemical Engineering & Equipment,2021(10):181-185., articleTitle=Failure analysis of lean methanol heat exchanger tube in the low‑temperature methanol wash unit, refAbstract=null), Reference(id=1324788959196356868, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2021, volume=50, issue=1, pageStart=125, pageEnd=126, url=null, language=null, rfNumber=3, rfOrder=4, authorNames=刘霞, 何鹏, journalName=山东化工, refType=null, unstructuredReference=刘霞,何鹏.低温甲醇洗装置腐蚀分析与处理[J].山东化工,2021,50(1):125-126., articleTitle=低温甲醇洗装置腐蚀分析与处理, refAbstract=null), Reference(id=1324788959271854341, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2021, volume=50, issue=1, pageStart=125, pageEnd=126, url=null, language=null, rfNumber=3, rfOrder=5, authorNames=LIU X, HE P, journalName=Shandong Chemical Industry, refType=null, unstructuredReference=LIU X,HE P.Corrosion analysis and treatment of low‑temperature methanol washing unit[J].Shandong Chemical Industry,2021,50(1):125-126., articleTitle=Corrosion analysis and treatment of low‑temperature methanol washing unit, refAbstract=null), Reference(id=1324788959347351814, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2023, volume=43, issue=11, pageStart=231, pageEnd=235, url=null, language=null, rfNumber=4, rfOrder=6, authorNames=王克华, 管凤宝, 夏祖虎, journalName=现代化工, refType=null, unstructuredReference=王克华,管凤宝,夏祖虎,等.煤制氢低温甲醇洗装置改造方案研究[J].现代化工,2023,43(11):231-235., articleTitle=煤制氢低温甲醇洗装置改造方案研究, refAbstract=null), Reference(id=1324788959414460679, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2023, volume=43, issue=11, pageStart=231, pageEnd=235, url=null, language=null, rfNumber=4, rfOrder=7, authorNames=WANG K H, GUAN F B, XIA Z H, journalName=Modern Chemical Industry, refType=null, unstructuredReference=WANG K H,GUAN F B,XIA Z H,et al.Research on upgrading scheme for rectisol unit in a coal to hydrogen plant[J].Modern Chemical Industry,2023,43(11):231-235., articleTitle=Research on upgrading scheme for rectisol unit in a coal to hydrogen plant, refAbstract=null), Reference(id=1324788959494152456, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2022, volume=null, issue=14, pageStart=118, pageEnd=121, url=null, language=null, rfNumber=5, rfOrder=8, authorNames=杨德忠, 张坤, 周明, journalName=化工管理, refType=null, unstructuredReference=杨德忠,张坤,周明.低温甲醇洗甲醇换热器腐蚀原因分析[J].化工管理,2022(14):118-121., articleTitle=低温甲醇洗甲醇换热器腐蚀原因分析, refAbstract=null), Reference(id=1324788959557067017, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2022, volume=null, issue=14, pageStart=118, pageEnd=121, url=null, language=null, rfNumber=5, rfOrder=9, authorNames=YANG D Z, ZHANG K, ZHOU M, journalName=Chemical Engineering Management, refType=null, unstructuredReference=YANG D Z,ZHANG K,ZHOU M.Analysis of corrosion causes of methanol heat exchanger[J].Chemical Engineering Management,2022(14):118-121., articleTitle=Analysis of corrosion causes of methanol heat exchanger, refAbstract=null), Reference(id=1324788959628370186, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2024, volume=41, issue=6, pageStart=73, pageEnd=82, url=null, language=null, rfNumber=6, rfOrder=10, authorNames=苏国庆, 李彦, 窦站, journalName=压力容器, refType=null, unstructuredReference=苏国庆,李彦,窦站,等.硫回收装置余热锅炉铵盐结晶腐蚀机理研究[J].压力容器,2024,41(6):73-82., articleTitle=硫回收装置余热锅炉铵盐结晶腐蚀机理研究, refAbstract=null), Reference(id=1324788959682896139, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2024, volume=41, issue=6, pageStart=73, pageEnd=82, url=null, language=null, rfNumber=6, rfOrder=11, authorNames=SU G Q, LI Y, DOU Z, journalName=Pressure Vessel Technology, refType=null, unstructuredReference=SU G Q,LI Y,DOU Z,et al.Study on the corrosion mechanism of ammonium salt crystallization in waste heat boiler of a sulphur recovery unit[J].Pressure Vessel Technology,2024,41(6):73-82., articleTitle=Study on the corrosion mechanism of ammonium salt crystallization in waste heat boiler of a sulphur recovery unit, refAbstract=null), Reference(id=1324788959745810700, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2024, volume=52, issue=10, pageStart=41, pageEnd=48, url=null, language=null, rfNumber=7, rfOrder=12, authorNames=陈聚凯, 吴肖文, 周慧, journalName=流体机械, refType=null, unstructuredReference=陈聚凯,吴肖文,周慧,等.基于CFD-DPM模拟的冷氢化工艺旋风分离器内气固两相流动及冲蚀磨损特性研究[J].流体机械,2024,52(10):41-48., articleTitle=基于CFD-DPM模拟的冷氢化工艺旋风分离器内气固两相流动及冲蚀磨损特性研究, refAbstract=null), Reference(id=1324788959804530957, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2024, volume=52, issue=10, pageStart=41, pageEnd=48, url=null, language=null, rfNumber=7, rfOrder=13, authorNames=CHEN J K, WU X W, ZHOU H, journalName=Fluid Machinery, refType=null, unstructuredReference=CHEN J K,WU X W,ZHOU H,et al.Study on characteristics of gas‑particle two‑phase flow and erosion in a cyclone separator used in cold hydrogenation process based on CFD-DPM modeling[J].Fluid Machinery,2024,52(10):41-48., articleTitle=Study on characteristics of gas‑particle two‑phase flow and erosion in a cyclone separator used in cold hydrogenation process based on CFD-DPM modeling, refAbstract=null), Reference(id=1324788959884222734, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2023, volume=51, issue=10, pageStart=10, pageEnd=17, url=null, language=null, rfNumber=8, rfOrder=14, authorNames=金浩哲, 陈凤官, 王超, journalName=流体机械, refType=null, unstructuredReference=金浩哲,陈凤官,王超,等.煤气化装置黑水阀冲蚀磨损机理及智能防控研究[J].流体机械,2023,51(10):10-17., articleTitle=煤气化装置黑水阀冲蚀磨损机理及智能防控研究, refAbstract=null), Reference(id=1324788959947137295, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2023, volume=51, issue=10, pageStart=10, pageEnd=17, url=null, language=null, rfNumber=8, rfOrder=15, authorNames=JIN H Z, CHEN F G, WANG C, journalName=Fluid Machinery, refType=null, unstructuredReference=JIN H Z,CHEN F G,WANG C,et al.Research on erosion wear mechanism and intelligent prevention and control of the black water valve in coal gasification plant[J].Fluid Machinery,2023,51(10):10-17., articleTitle=Research on erosion wear mechanism and intelligent prevention and control of the black water valve in coal gasification plant, refAbstract=null), Reference(id=1324788960022634768, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2024, volume=52, issue=10, pageStart=74, pageEnd=81, url=null, language=null, rfNumber=9, rfOrder=16, authorNames=刘忠伟, 苗超, 何萌, journalName=流体机械, refType=null, unstructuredReference=刘忠伟,苗超,何萌,等.催化裂化提升管T型出口气固两相流冲蚀研究[J].流体机械,2024,52(10):74-81., articleTitle=催化裂化提升管T型出口气固两相流冲蚀研究, refAbstract=null), Reference(id=1324788960089743633, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2024, volume=52, issue=10, pageStart=74, pageEnd=81, url=null, language=null, rfNumber=9, rfOrder=17, authorNames=LIU Z W, MIAO C, HE M, journalName=Fluid Machinery, refType=null, unstructuredReference=LIU Z W,MIAO C,HE M,et al.Study on erosion of gas-solid two‑phase flow at T‑type outlet of FCC riser[J].Fluid Machinery,2024,52(10):74-81., articleTitle=Study on erosion of gas-solid two‑phase flow at T‑type outlet of FCC riser, refAbstract=null), Reference(id=1324788960161046802, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2023, volume=41, issue=5, pageStart=46, pageEnd=51, url=null, language=null, rfNumber=10, rfOrder=18, authorNames=葛伟伟, 李庆昕, 赵鑫鑫, journalName=包装与食品机械, refType=null, unstructuredReference=葛伟伟,李庆昕,赵鑫鑫,等.陶瓷强化涂层在饮料灌装机中的应用[J].包装与食品机械,2023,41(5):46-51., articleTitle=陶瓷强化涂层在饮料灌装机中的应用, refAbstract=null), Reference(id=1324788960236544275, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2023, volume=41, issue=5, pageStart=46, pageEnd=51, url=null, language=null, rfNumber=10, rfOrder=19, authorNames=GE W W, LI Q X, ZHAO X X, journalName=Packaging and Food Machinery, refType=null, unstructuredReference=GE W W,LI Q X,ZHAO X X,et al.Application of ceramic strengthening coating in beverage filling machine[J].Packaging and Food Machinery,2023,41(5):46-51., articleTitle=Application of ceramic strengthening coating in beverage filling machine, refAbstract=null), Reference(id=1324788960303653140, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2020, volume=48, issue=1, pageStart=64, pageEnd=66, url=null, language=null, rfNumber=11, rfOrder=20, authorNames=霍跃光, 赵小波, 邓金泉, journalName=煤化工, refType=null, unstructuredReference=霍跃光,赵小波,邓金泉.低温甲醇洗系统贫富甲醇换热器泄漏原因分析及处理[J].煤化工,2020,48(1):64-66., articleTitle=低温甲醇洗系统贫富甲醇换热器泄漏原因分析及处理, refAbstract=null), Reference(id=1324788960383344917, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2020, volume=48, issue=1, pageStart=64, pageEnd=66, url=null, language=null, rfNumber=11, rfOrder=21, authorNames=HUO Y G, ZHAO X B, DENG J Q, journalName=Coal Chemical Industry, refType=null, unstructuredReference=HUO Y G,ZHAO X B,DENG J Q.Analysis and treatment of leakage of lean‑rich methanol heat exchanger for the low‑temperature methanol washing system[J].Coal Chemical Industry,2020,48(1): 64-66., articleTitle=Analysis and treatment of leakage of lean‑rich methanol heat exchanger for the low‑temperature methanol washing system, refAbstract=null), Reference(id=1324788960450453782, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2022, volume=21, issue=1, pageStart=67, pageEnd=69, url=null, language=null, rfNumber=12, rfOrder=22, authorNames=张红卫, 张武, journalName=宁夏工程技术, refType=null, unstructuredReference=张红卫,张武.低温甲醇洗绕管式换热器泄漏原因及处理措施[J].宁夏工程技术,2022,21(1):67-69., articleTitle=低温甲醇洗绕管式换热器泄漏原因及处理措施, refAbstract=null), Reference(id=1324788962132369687, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2022, volume=21, issue=1, pageStart=67, pageEnd=69, url=null, language=null, rfNumber=12, rfOrder=23, authorNames=ZHUANG H W, ZHANG W, journalName=Ningxia Engineering Technology, refType=null, unstructuredReference=ZHUANG H W,ZHANG W.Analysis of leakage causes and solutions of the cleaning of spiral wound heat exchanger in rectisol unit[J].Ningxia Engineering Technology,2022,21(1):67-69., articleTitle=Analysis of leakage causes and solutions of the cleaning of spiral wound heat exchanger in rectisol unit, refAbstract=null), Reference(id=1324788962224644376, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2017, volume=43, issue=9, pageStart=52, pageEnd=53, url=null, language=null, rfNumber=13, rfOrder=24, authorNames=陈志明, journalName=内蒙古石油化工, refType=null, unstructuredReference=陈志明.低温甲醇洗换热器腐蚀问题浅析[J].内蒙古石油化工,2017,43(9):52-53., articleTitle=低温甲醇洗换热器腐蚀问题浅析, refAbstract=null), Reference(id=1324788962283364633, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2017, volume=43, issue=9, pageStart=52, pageEnd=53, url=null, language=null, rfNumber=13, rfOrder=25, authorNames=CHEN Z M, journalName=Inner Mongolia Petrochemical Industry, refType=null, unstructuredReference=CHEN Z M.A brief analysis of the corrosion issues in low‑temperature methanol wash heat exchangers[J].Inner Mongolia Petrochemical Industry,2017,43(9):52-53., articleTitle=A brief analysis of the corrosion issues in low‑temperature methanol wash heat exchangers, refAbstract=null), Reference(id=1324788962363056410, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2016, volume=null, issue=null, pageStart=null, pageEnd=null, url=null, language=null, rfNumber=14, rfOrder=26, authorNames=张玉福, journalName=null, refType=null, unstructuredReference=张玉福.多介质环境下压力容器用材腐蚀失效机理研究[D].兰州:兰州理工大学,2016., articleTitle=多介质环境下压力容器用材腐蚀失效机理研究, refAbstract=null), Reference(id=1324788962425970971, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2016, volume=null, issue=null, pageStart=null, pageEnd=null, url=null, language=null, rfNumber=14, rfOrder=27, authorNames=ZHANG Y F, journalName=null, refType=null, unstructuredReference=ZHANG Y F.The research on the corrosion failure mechanism of pressure vessel materials under multi‑media environment[D].Lanzhou:Lanzhou University of Technology,2016., articleTitle=The research on the corrosion failure mechanism of pressure vessel materials under multi‑media environment, refAbstract=null), Reference(id=1324788962501468444, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2018, volume=47, issue=12, pageStart=21, pageEnd=29, url=null, language=null, rfNumber=15, rfOrder=28, authorNames=冯桓榰, 邢希金, 谷林, journalName=表面技术, refType=null, unstructuredReference=冯桓榰,邢希金,谷林,等.高温高压高含硫气井T95技术套管腐蚀实验研究[J].表面技术,2018,47(12):21-29., articleTitle=高温高压高含硫气井T95技术套管腐蚀实验研究, refAbstract=null), Reference(id=1324788962585354525, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2018, volume=47, issue=12, pageStart=21, pageEnd=29, url=null, language=null, rfNumber=15, rfOrder=29, authorNames=FENG H Z, XING X J, GU L, journalName=Surface Technology, refType=null, unstructuredReference=FENG H Z,XING X J,GU L,et al.Corrosion behavior of T95 casing in high temperature,high pressure and high H2S condition[J].Surface Technology,2018,47(12):21-29., articleTitle=Corrosion behavior of T95 casing in high temperature,high pressure and high H2S condition, refAbstract=null), Reference(id=1324788962648269086, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2007, volume=null, issue=5, pageStart=121, pageEnd=123, url=null, language=null, rfNumber=16, rfOrder=30, authorNames=胡兴民, 朱天寿, 张书成, journalName=天然气工业, refType=null, unstructuredReference=胡兴民,朱天寿,张书成,等.靖边气田天然气脱硫装置腐蚀行为研究[J].天然气工业,2007(5):121-123., articleTitle=靖边气田天然气脱硫装置腐蚀行为研究, refAbstract=null), Reference(id=1324788962719572255, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2007, volume=null, issue=5, pageStart=121, pageEnd=123, url=null, language=null, rfNumber=16, rfOrder=31, authorNames=HU X M, ZHU T S, ZHANG S C, journalName=Natural Gas Industry, refType=null, unstructuredReference=HU X M,ZHU T S,ZHANG S C,et al.Corrosion performance study on natural gas desulfurization unit in the Jingbian gas field[J].Natural Gas Industry,2007(5):121-123., articleTitle=Corrosion performance study on natural gas desulfurization unit in the Jingbian gas field, refAbstract=null), Reference(id=1324788962774098208, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2005, volume=null, issue=null, pageStart=null, pageEnd=null, url=null, language=null, rfNumber=17, rfOrder=32, authorNames=李春福, journalName=null, refType=null, unstructuredReference=李春福.油气开发过程中的CO2腐蚀机理及防护技术研究[D].成都:西南石油学院,2005., articleTitle=油气开发过程中的CO2腐蚀机理及防护技术研究, refAbstract=null), Reference(id=1324788962849595681, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2005, volume=null, issue=null, pageStart=null, pageEnd=null, url=null, language=null, rfNumber=17, rfOrder=33, authorNames=LI C F, journalName=null, refType=null, unstructuredReference=LI C F.Research on CO2 corrosion mechanism and protection technology in oil and gas development process[D].Chengdu:Southwest Petroleum Institute,2005., articleTitle=Research on CO2 corrosion mechanism and protection technology in oil and gas development process, refAbstract=null), Reference(id=1324788962912510242, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2019, volume=null, issue=null, pageStart=null, pageEnd=null, url=null, language=null, rfNumber=18, rfOrder=34, authorNames=李慧心, journalName=null, refType=null, unstructuredReference=李慧心.高含H2S环境下低合金钢腐蚀产物演化及其对腐蚀行为的影响[D].北京:北京科技大学,2019., articleTitle=高含H2S环境下低合金钢腐蚀产物演化及其对腐蚀行为的影响, refAbstract=null), Reference(id=1324788962979619107, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2019, volume=null, issue=null, pageStart=null, pageEnd=null, url=null, language=null, rfNumber=18, rfOrder=35, authorNames=LI H X, journalName=null, refType=null, unstructuredReference=LI H X.Formation and evolution of H2S corrosion products and the influence on corrosion mechanism under high H2S partial pressure[D].Beijing:Beijing University of Science and Technology,2019., articleTitle=Formation and evolution of H2S corrosion products and the influence on corrosion mechanism under high H2S partial pressure, refAbstract=null), Reference(id=1324788963038339364, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2020, volume=48, issue=9, pageStart=14, pageEnd=19, url=null, language=null, rfNumber=19, rfOrder=36, authorNames=管晨羽, 李燕, 张述伟, journalName=化学工程, refType=null, unstructuredReference=管晨羽,李燕,张述伟.某厂低温甲醇洗中杂质硫的影响及消除研究[J].化学工程,2020,48(9):14-19., articleTitle=某厂低温甲醇洗中杂质硫的影响及消除研究, refAbstract=null), Reference(id=1324788963105448229, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2020, volume=48, issue=9, pageStart=14, pageEnd=19, url=null, language=null, rfNumber=19, rfOrder=37, authorNames=GUAN C Y, LI Y, ZHANG S W, journalName=Chemical Engineering (China), refType=null, unstructuredReference=GUAN C Y,LI Y,ZHANG S W.Study on influence and elimination of sulfide impurities in chilled methanol wash process of a plant[J].Chemical Engineering (China),2020,48(9):14-19., articleTitle=Study on influence and elimination of sulfide impurities in chilled methanol wash process of a plant, refAbstract=null), Reference(id=1324788963197722918, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2023, volume=52, issue=2, pageStart=148, pageEnd=157, url=null, language=null, rfNumber=20, rfOrder=38, authorNames=贺三, 罗斯琪, 赵浩童, journalName=表面技术, refType=null, unstructuredReference=贺三,罗斯琪,赵浩童,等.碳钢在CO2环境中无机垢下腐蚀研究进展[J].表面技术,2023,52(2):148-157., articleTitle=碳钢在CO2环境中无机垢下腐蚀研究进展, refAbstract=null), Reference(id=1324788963269026087, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2023, volume=52, issue=2, pageStart=148, pageEnd=157, url=null, language=null, rfNumber=20, rfOrder=39, authorNames=HE S, LUO S Q, ZHAO H T, journalName=Surface Technology, refType=null, unstructuredReference=HE S,LUO S Q,ZHAO H T,et al.Review of carbon steel under deposit corrosion in CO2 environment[J].Surface Technology,2023,52(2):148-157., articleTitle=Review of carbon steel under deposit corrosion in CO2 environment, refAbstract=null), Reference(id=1324788963340329256, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2019, volume=40, issue=11, pageStart=810, pageEnd=815, url=null, language=null, rfNumber=21, rfOrder=40, authorNames=范金福, 刘猛, 张晓辰, journalName=腐蚀与防护, refType=null, unstructuredReference=范金福,刘猛,张晓辰,等.流速对垢下腐蚀的影响及其腐蚀机理[J].腐蚀与防护,2019,40(11):810-815., articleTitle=流速对垢下腐蚀的影响及其腐蚀机理, refAbstract=null), Reference(id=1324788963424215337, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2019, volume=40, issue=11, pageStart=810, pageEnd=815, url=null, language=null, rfNumber=21, rfOrder=41, authorNames=FAN J F, LIU M, ZHANG X C, journalName=Corrosion & Protection, refType=null, unstructuredReference=FAN J F,LIU M,ZHANG X C,et al.Effect of velocity on the under‑deposit corrosion and its corrosion mechanism[J].Corrosion & Protection,2019,40(11):810-815., articleTitle=Effect of velocity on the under‑deposit corrosion and its corrosion mechanism, refAbstract=null), Reference(id=1324788963520684330, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2023, volume=40, issue=4, pageStart=59, pageEnd=66, url=null, language=null, rfNumber=22, rfOrder=42, authorNames=郭福平, 吕运容, 段志宏, journalName=压力容器, refType=null, unstructuredReference=郭福平,吕运容,段志宏,等.重整装置双相不锈钢换热器腐蚀泄漏原因分析[J].压力容器,2023,40(4):59-66., articleTitle=重整装置双相不锈钢换热器腐蚀泄漏原因分析, refAbstract=null), Reference(id=1324788963600376107, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2023, volume=40, issue=4, pageStart=59, pageEnd=66, url=null, language=null, rfNumber=22, rfOrder=43, authorNames=GUO F P, LYU Y R, DUAN Z H, journalName=Pressure Vessel Technology, refType=null, unstructuredReference=GUO F P,LYU Y R,DUAN Z H,et al.Analysis on corrosion leakage cause of duplex stainless steel heat exchanger in a catalytic reforming unit[J].Pressure Vessel Technology,2023,40(4):59-66., articleTitle=Analysis on corrosion leakage cause of duplex stainless steel heat exchanger in a catalytic reforming unit, refAbstract=null), Reference(id=1324788963659096364, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2017, volume=50, issue=2, pageStart=74, pageEnd=77, url=null, language=null, rfNumber=23, rfOrder=44, authorNames=蒋志国, 王辉煌, 龚利华, journalName=材料保护, refType=null, unstructuredReference=蒋志国,王辉煌,龚利华,等.Cl-和H2S对不锈钢电化学行为的协同影响[J].材料保护,2017,50(2):74-77., articleTitle=Cl-和H2S对不锈钢电化学行为的协同影响, refAbstract=null), Reference(id=1324788963742982445, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, doi=null, pmid=null, pmcid=null, year=2017, volume=50, issue=2, pageStart=74, pageEnd=77, url=null, language=null, rfNumber=23, rfOrder=45, authorNames=JIANG Z G, WANG H H, GONG L H, journalName=Materials Protection, refType=null, unstructuredReference=JIANG Z G,WANG H H,GONG L H,et al.Combined effects of Cl- and H2S on electrochemical behavior of stainless stee[J].Materials Protection,2017,50(2):74-77., articleTitle=Combined effects of Cl- and H2S on electrochemical behavior of stainless stee, refAbstract=null)], funds=[Fund(id=1324788958781120767, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, awardId=null, language=CN, fundingSource=国家重点研发计划项目(2021YFB3301100);北京化工大学交叉学科项目(XK2023-07), fundOrder=null, country=null)], companyList=[AuthorCompany(id=1324788951541752001, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, xref=1, ext=[AuthorCompanyExt(id=1324788951550140610, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788951541752001, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1College of Mechanical and Electrical Engineering,Beijing University of Chemical Technology,Beijing 100029,China), AuthorCompanyExt(id=1324788951558529219, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788951541752001, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1北京化工大学 机电工程学院,北京 100029)]), AuthorCompany(id=1324788953139781828, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, xref=2, ext=[AuthorCompanyExt(id=1324788953148170437, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788953139781828, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=2National Energy Group Ningxia Coal Industry Co.,Ltd.,Coal to Oil Branch,Yinchuan 750411,China), AuthorCompanyExt(id=1324788953156559046, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788953139781828, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=2国家能源集团 宁夏煤业有限责任公司 煤制油分公司,银川 750411)])], figs=[ArticleFig(id=1324788955069161701, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=EN, label=Fig.1, caption=Process flow schematic of a low‑temperature methanol washing units, figureFileSmall=iix9h6Nj83GHnbESKlS+SA==, figureFileBig=LPaM00CoHvmh+6QOvyCMzQ==, tableContent=null), ArticleFig(id=1324788955169824998, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=CN, label=图1, caption=低温甲醇洗装置的工艺流程示意, figureFileSmall=iix9h6Nj83GHnbESKlS+SA==, figureFileBig=LPaM00CoHvmh+6QOvyCMzQ==, tableContent=null), ArticleFig(id=1324788955362762983, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=EN, label=Fig.2, caption=Corrosion morphology in different regions of heat exchangers, figureFileSmall=UjZLogh2xI1FTP+9Wsvn2Q==, figureFileBig=j0L/vWebasJjXO5KKfAC4g==, tableContent=null), ArticleFig(id=1324788955421483240, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=CN, label=图2, caption=换热器不同部位的腐蚀形貌

(a)进口封头  (b)出口封头处污泥  (c)管板

, figureFileSmall=UjZLogh2xI1FTP+9Wsvn2Q==, figureFileBig=j0L/vWebasJjXO5KKfAC4g==, tableContent=null), ArticleFig(id=1324788955480203497, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=EN, label=Fig.3, caption=Failure heat exchanger tubes, figureFileSmall=mZzJiSTzFCaJscpohSCG0g==, figureFileBig=4y00e79qV5KMfQrkgPwX2Q==, tableContent=null), ArticleFig(id=1324788955538923754, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=CN, label=图3, caption=失效换热管

(a)泄漏失效的换热管  (b)换热管内表面

, figureFileSmall=mZzJiSTzFCaJscpohSCG0g==, figureFileBig=4y00e79qV5KMfQrkgPwX2Q==, tableContent=null), ArticleFig(id=1324788955622809835, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=EN, label=Fig.4, caption=Microstructure of the sample, figureFileSmall=0LzKDFzVSV7j9Mh9iHw2hw==, figureFileBig=j6iAbd6y8BXc+7ZHrfN9BQ==, tableContent=null), ArticleFig(id=1324788955681530092, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=CN, label=图4, caption=样品的微观形貌, figureFileSmall=0LzKDFzVSV7j9Mh9iHw2hw==, figureFileBig=j6iAbd6y8BXc+7ZHrfN9BQ==, tableContent=null), ArticleFig(id=1324788955757027565, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=EN, label=Fig.5, caption=XRD results of the sample, figureFileSmall=z9D0ZNRa/ek/UdYWR2nmVw==, figureFileBig=9BT3SHg6z7HEYcduDReX3A==, tableContent=null), ArticleFig(id=1324788955815747822, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=CN, label=图5, caption=样品的X射线衍射结果, figureFileSmall=z9D0ZNRa/ek/UdYWR2nmVw==, figureFileBig=9BT3SHg6z7HEYcduDReX3A==, tableContent=null), ArticleFig(id=1324788955882856687, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=EN, label=Fig.6, caption=Treatment process of sludge samples, figureFileSmall=W4GQ61f8JPqoqXinZh8euw==, figureFileBig=gaN3ab+gABckFsCTRqF40g==, tableContent=null), ArticleFig(id=1324788955954159856, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=CN, label=图6, caption=污泥样品的处理过程

(a)黑色污泥  (b)污泥经800 ℃焚烧后  (c)污泥焚烧后研磨为粉末

, figureFileSmall=W4GQ61f8JPqoqXinZh8euw==, figureFileBig=gaN3ab+gABckFsCTRqF40g==, tableContent=null), ArticleFig(id=1324788956008685809, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=EN, label=Fig.7, caption=The micro‑corrosion morphology of the samples at different temperatures, figureFileSmall=m0Jx/GYUZ+RjfaqxEkEqMQ==, figureFileBig=mr2CHhjl8u5tESV9Ide61A==, tableContent=null), ArticleFig(id=1324788957715767538, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=CN, label=图7, caption=不同温度下试样的微观腐蚀形貌, figureFileSmall=m0Jx/GYUZ+RjfaqxEkEqMQ==, figureFileBig=mr2CHhjl8u5tESV9Ide61A==, tableContent=null), ArticleFig(id=1324788957782876403, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=EN, label=Fig.8, caption=The average corrosion rate of the samples at different temperatures, figureFileSmall=hYIZIHkXe35fdq16GMXaTw==, figureFileBig=BvitgqaEJtjERK+c7GbWiA==, tableContent=null), ArticleFig(id=1324788957841596660, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=CN, label=图8, caption=不同温度下试样的平均腐蚀速率, figureFileSmall=hYIZIHkXe35fdq16GMXaTw==, figureFileBig=BvitgqaEJtjERK+c7GbWiA==, tableContent=null), ArticleFig(id=1324788957950648565, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=EN, label=Fig.9, caption=Mechanism of under‑deposit corrosion of heat exchange tubes, figureFileSmall=pI8SIMmq1LAIpddgw36N4g==, figureFileBig=L7m8QXU8+RPmY74iWeGdFw==, tableContent=null), ArticleFig(id=1324788958034534646, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=CN, label=图9, caption=换热管垢下腐蚀的机理示意, figureFileSmall=pI8SIMmq1LAIpddgw36N4g==, figureFileBig=L7m8QXU8+RPmY74iWeGdFw==, tableContent=null), ArticleFig(id=1324788958135197943, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=EN, label=Tab.1, caption=

Process parameters of the heat exchanger

, figureFileSmall=null, figureFileBig=null, tableContent=
项目管程壳程
介质类型富硫甲醇贫硫甲醇
进/出口温度/℃28/8794/40
压力/MPa1.20.25
), ArticleFig(id=1324788958248444152, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=CN, label=表1, caption=

换热器的工艺参数

, figureFileSmall=null, figureFileBig=null, tableContent=
项目管程壳程
介质类型富硫甲醇贫硫甲醇
进/出口温度/℃28/8794/40
压力/MPa1.20.25
), ArticleFig(id=1324788958315553017, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=EN, label=Tab.2, caption=

Equipment parameters of the heat exchanger

, figureFileSmall=null, figureFileBig=null, tableContent=
项目参数
型式管壳式
管程材质10钢
壳程材质Q245R
换热管规格⌀25 mm×2.5 mm
), ArticleFig(id=1324788958395244794, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=CN, label=表2, caption=

换热器的设备参数

, figureFileSmall=null, figureFileBig=null, tableContent=
项目参数
型式管壳式
管程材质10钢
壳程材质Q245R
换热管规格⌀25 mm×2.5 mm
), ArticleFig(id=1324788958474936571, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=EN, label=Tab.3, caption=

EDS results of the sample

, figureFileSmall=null, figureFileBig=null, tableContent=
元素点1点2点3
Fe37.440.143.6
S24.022.326.8
C18.417.014.4
O20.120.615.2
), ArticleFig(id=1324788958546239740, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=CN, label=表3, caption=

样品的能谱结果

, figureFileSmall=null, figureFileBig=null, tableContent=
元素点1点2点3
Fe37.440.143.6
S24.022.326.8
C18.417.014.4
O20.120.615.2
), ArticleFig(id=1324788958609154301, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=EN, label=Tab.4, caption=

Oxide analysis results of mastic samples

, figureFileSmall=null, figureFileBig=null, tableContent=
项目Fe2O3NiOSO3MnOCaOSiO2MgOMoO3TiO2ZnO
焚烧前60.991.0137.0300.180.200.140.130.0120.020.04
焚烧后96.381.730.4540.290.300.250.140.0200.040.08
), ArticleFig(id=1324788958672068862, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, language=CN, label=表4, caption=

污泥样品的氧化物分析结果

, figureFileSmall=null, figureFileBig=null, tableContent=
项目Fe2O3NiOSO3MnOCaOSiO2MgOMoO3TiO2ZnO
焚烧前60.991.0137.0300.180.200.140.130.0120.020.04
焚烧后96.381.730.4540.290.300.250.140.0200.040.08
)], attaches=null, journal=Journal(id=1319354845020389520, delFlag=0, nameCn=压力容器, nameEn=Pressure Vessel Technology, nameHistory1=null, nameHistory2=null, issn=1001-4837, eissn=null, cn=34-1058/TH, coden=null, periodic=0, language=CN, oaType=null, ccby=null, superviseOffice=null, ownerOffice=null, pubOffice=null, editorOffice=null, officeType=null, aims=null, clcCode=null, officeProv=null, officeCity=null, officeAddr=null, officeZip=null, officeEmail=null, officePhone=null, editDirector=null, officeDirector=null, officeDirectorPhone=null, officeStaffNum=null, officeEmpNum=null, coverPicUrl=jxjNdnQvHSQ8b9q0zS7Bgw==, journalPrice=null, startedYear=null, abbrevIsoEn=Pressure Vessel Technology, journalRemark=null, publicationField=null, createdTime=1792488307482, updatedTime=1792488496537, createdBy=18614031015, updatedBy=13701087609, firstLetterCn=Y, firstLetterEn=Y, subjectCode=Engineering, subjectName=null, subjectCodeEn=Engineering, subjectNameEn=null, picCn=jxjNdnQvHSQ8b9q0zS7Bgw==, picEn=4fVBwqRFt4uCO8g42aXObg==, jcr=null, cjcr=null, exts=[JournalExt(id=1319355638048740090, language=CN, name=压力容器, nameHistory1=null, nameHistory2=null, managedBy=, sponsoredBy=, publishedBy=, editorOffice=, officeProv=null, officeCity=null, officeAddr=, officeZip=, editDirector=, officeDirector=null, officePhone=null, coverPicUrl=null, journalRemark=, submitArticleUrl=null, websiteUrl=, createdTime=1792488496553, updatedTime=1792488496553, createdBy=13701087609, updatedBy=13701087609, submissionGuidelinesUrl=, submissionAuthorUrl=https://ylrq.portal.founderss.cn, submissionEditorUrl=https://journal.ids.fzyun.cn, submissionReviewUrl=https://ylrq.portal.founderss.cn, submissionCeEditorUrl=, submissionAeEditorUrl=, option={"copyright":""}), JournalExt(id=1319355638103266043, language=EN, name=Pressure Vessel Technology, nameHistory1=null, nameHistory2=null, managedBy=, sponsoredBy=, publishedBy=, editorOffice=, officeProv=null, officeCity=null, officeAddr=, officeZip=, editDirector=, officeDirector=null, officePhone=null, coverPicUrl=null, journalRemark=, submitArticleUrl=null, websiteUrl=, createdTime=1792488496566, updatedTime=1792488496566, createdBy=13701087609, updatedBy=13701087609, submissionGuidelinesUrl=, submissionAuthorUrl=https://ylrq.portal.founderss.cn, submissionEditorUrl=https://journal.ids.fzyun.cn, submissionReviewUrl=https://ylrq.portal.founderss.cn, submissionCeEditorUrl=, submissionAeEditorUrl=, option={"copyright":""})], databaseList=null, tenantJournalId=1319355204128309394, websiteList=[Website(id=1319376331645764504, webName=null, webTitle=null, webDomain=null, webCopyrigh=null, webIpcNo=null, seoTitle=null, seoKeywords=null, seoDescription=null, tenantJournalId=null, journalId=1319355204128309394, journalNameCn=null, journalNameEn=null, grayFlag=null, tenantId=1146029695717560320, platformId=null, journalGroupId=null, journalGroupNameCn=null, journalGroupNameEn=null, type=1, domain=https://castjournals.cast.org.cn/joweb/ylrq/CN, language=CN, createTime=1792493430291, createBy=18614031015, updateTime=1792493471510, updateBy=18614031015, name=压力容器-中文, tplId=1146099689490845704, title=压力容器, delFlag=0, indexPage=/home, props=[WebsiteProps(id=1319376610952856568, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=articleTextType, value=kx, createTime=1792493496883, updateTime=1792493496883, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610923496437, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=banner, value=null, createTime=1792493496876, updateTime=1792493496876, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610969633787, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=grayFlag, value=0, createTime=1792493496887, updateTime=1792493496887, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610910913524, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=logo, value=https://castjournals.cast.org.cn/joweb/ylrq/CN/file/pic?fileId=jTQ3ULyAlxRu0s8fI4nfng==, createTime=1792493496873, updateTime=1792493496873, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610986411005, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=minRunFlag, value=0, createTime=1792493496891, updateTime=1792493496891, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610944467959, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=picServerUrl, value=https://castjournals.cast.org.cn/joweb/ylrq/CN/file/pic, createTime=1792493496881, updateTime=1792493496881, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610978022396, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=silenceFlag, value=0, createTime=1792493496889, updateTime=1792493496889, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610936079350, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=staticResourcePath, value=https://castjournals.cast.org.cn/joweb/cast_kjdb_cn_619/, createTime=1792493496879, updateTime=1792493496879, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610957050873, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=themeColor, value=null, createTime=1792493496884, updateTime=1792493496884, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610965439482, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=themeStyle, value=null, createTime=1792493496886, updateTime=1792493496886, creator=18614031015, updator=18614031015)]), Website(id=1319376331893228450, webName=null, webTitle=null, webDomain=null, webCopyrigh=null, webIpcNo=null, seoTitle=null, seoKeywords=null, seoDescription=null, tenantJournalId=null, journalId=1319355204128309394, journalNameCn=null, journalNameEn=null, grayFlag=null, tenantId=1146029695717560320, platformId=null, journalGroupId=null, journalGroupNameCn=null, journalGroupNameEn=null, type=1, domain=https://castjournals.cast.org.cn/joweb/ylrq/EN, language=EN, createTime=1792493430350, createBy=18614031015, updateTime=1792493467616, updateBy=18614031015, name=压力容器-英文, tplId=1146101810881728533, title=Pressure Vessel Technology, delFlag=0, indexPage=/home, props=[WebsiteProps(id=1319376586462315499, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=articleTextType, value=kx, createTime=1792493491044, updateTime=1792493491044, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586432955368, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=banner, value=null, createTime=1792493491037, updateTime=1792493491037, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586500064238, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=grayFlag, value=0, createTime=1792493491053, updateTime=1792493491053, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586420372455, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=logo, value=https://castjournals.cast.org.cn/joweb/ylrq/EN/file/pic?fileId=jTQ3ULyAlxRu0s8fI4nfng==, createTime=1792493491034, updateTime=1792493491034, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586521035760, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=minRunFlag, value=0, createTime=1792493491058, updateTime=1792493491058, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586453926890, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=picServerUrl, value=https://castjournals.cast.org.cn/joweb/ylrq/EN/file/pic, createTime=1792493491042, updateTime=1792493491042, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586512647151, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=silenceFlag, value=0, createTime=1792493491056, updateTime=1792493491056, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586441343977, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=staticResourcePath, value=https://castjournals.cast.org.cn/joweb/cast_kjdb_en_623/, createTime=1792493491039, updateTime=1792493491039, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586474898412, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=themeColor, value=null, createTime=1792493491047, updateTime=1792493491047, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586487481325, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=themeStyle, value=null, createTime=1792493491050, updateTime=1792493491050, creator=18614031015, updator=18614031015)])], journalTitle=压力容器, weixinUrl=null, journalUrl=https://www.pvtjournal.com/, iacademicId=null, status=1, seqNo=null, journalTitleEn=Pressure Vessel Technology, journalPhotoCn=jxjNdnQvHSQ8b9q0zS7Bgw==, journalPhotoEn=4fVBwqRFt4uCO8g42aXObg==, journalFirstLetter=Y, journalRecommend=null, journalNew=null, journalCollection=null, jcrJf=null, cjcrJf=null, jcrJfStr=null, cjcrJfStr=null, submissionFirstDecision=null, sciSubjectClassification=null, casSubjectClassification=null, citeScore=null, totalCitationFrequency=null, icpCode=null, psCode=null, advertisingLicenseCode=null, copyrightInformation=null, country=null, option=, provinceCode=null, provinceName=null, collectFlag=false, interPubPlatform=, interPubPlatformUrl=null), detailUrlCn=https://castjournals.cast.org.cn/joweb/ylrq/CN/10.3969/j.issn.1001-4837.2025.03.009, detailUrlEn=https://castjournals.cast.org.cn/joweb/ylrq/EN/10.3969/j.issn.1001-4837.2025.03.009, pdfUrlCn=https://castjournals.cast.org.cn/joweb/ylrq/CN/PDF/10.3969/j.issn.1001-4837.2025.03.009, pdfUrlEn=https://castjournals.cast.org.cn/joweb/ylrq/EN/PDF/10.3969/j.issn.1001-4837.2025.03.009, aliStartDate=0, aliEndDate=0, collectionFlag=false, citedCount=null, citedUrl=null, previewStatus=0, delFlag=0, hasFullText=1, orderTime=1743264000000, fullTextJson=null, articleText=null, reference=null)
收藏切换
低温甲醇洗装置换热器腐蚀泄漏原因分析
苏国庆 1 , 李彦 1 , 张建文 1 , 张志军 2
压力容器 | 安全分析 2025,42(3): 71-78
收起
收藏切换
压力容器 |安全分析 2025 , 42 (3) : 71 -78
低温甲醇洗装置换热器腐蚀泄漏原因分析
全屏
[Author(id=1324788953219473608, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, orderNo=0, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=1556544322@qq.com, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1324788953328525514, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, authorId=1324788953219473608, language=EN, stringName=Guoqing SU, firstName=Guoqing, middleName=null, lastName=SU, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1College of Mechanical and Electrical Engineering,Beijing University of Chemical Technology,Beijing 100029,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1324788953395634379, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, authorId=1324788953219473608, language=CN, stringName=苏国庆, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1北京化工大学 机电工程学院,北京 100029, bio={"content":"

苏国庆(1994),男,主要研究方向为多相流腐蚀,通信地址:100029北京市朝阳区北三环东路15号北京化工大学机电工程学院,E-mail:。

"}, bioImg=null, bioContent=

苏国庆(1994),男,主要研究方向为多相流腐蚀,通信地址:100029北京市朝阳区北三环东路15号北京化工大学机电工程学院,E-mail:。

, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1324788951541752001, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, xref=1, ext=[AuthorCompanyExt(id=1324788951550140610, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788951541752001, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1College of Mechanical and Electrical Engineering,Beijing University of Chemical Technology,Beijing 100029,China), AuthorCompanyExt(id=1324788951558529219, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788951541752001, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1北京化工大学 机电工程学院,北京 100029)])]), Author(id=1324788953487909069, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, orderNo=1, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1324788953571795151, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, authorId=1324788953487909069, language=EN, stringName=Yan LI, firstName=Yan, middleName=null, lastName=LI, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1College of Mechanical and Electrical Engineering,Beijing University of Chemical Technology,Beijing 100029,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1324788953638904016, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, authorId=1324788953487909069, language=CN, stringName=李彦, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1北京化工大学 机电工程学院,北京 100029, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1324788951541752001, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, xref=1, ext=[AuthorCompanyExt(id=1324788951550140610, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788951541752001, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1College of Mechanical and Electrical Engineering,Beijing University of Chemical Technology,Beijing 100029,China), AuthorCompanyExt(id=1324788951558529219, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788951541752001, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1北京化工大学 机电工程学院,北京 100029)])]), Author(id=1324788953710207186, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, orderNo=2, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=zhangjw@mail.buct.edu.cn, emailSecond=null, emailThird=null, correspondingAuthor=1, authorType=1, ext={EN=AuthorExt(id=1324788953789898964, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, authorId=1324788953710207186, language=EN, stringName=Jianwen ZHANG, firstName=Jianwen, middleName=null, lastName=ZHANG, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1College of Mechanical and Electrical Engineering,Beijing University of Chemical Technology,Beijing 100029,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1324788953873785045, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, authorId=1324788953710207186, language=CN, stringName=张建文, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1北京化工大学 机电工程学院,北京 100029, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1324788951541752001, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, xref=1, ext=[AuthorCompanyExt(id=1324788951550140610, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788951541752001, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1College of Mechanical and Electrical Engineering,Beijing University of Chemical Technology,Beijing 100029,China), AuthorCompanyExt(id=1324788951558529219, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788951541752001, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1北京化工大学 机电工程学院,北京 100029)])]), Author(id=1324788953945088215, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, orderNo=3, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1324788954008002777, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, authorId=1324788953945088215, language=EN, stringName=Zhijun ZHANG, firstName=Zhijun, middleName=null, lastName=ZHANG, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=2, address=2National Energy Group Ningxia Coal Industry Co.,Ltd.,Coal to Oil Branch,Yinchuan 750411,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1324788954075111642, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, authorId=1324788953945088215, language=CN, stringName=张志军, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=2, address=2国家能源集团 宁夏煤业有限责任公司 煤制油分公司,银川 750411, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1324788953139781828, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, xref=2, ext=[AuthorCompanyExt(id=1324788953148170437, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788953139781828, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=2National Energy Group Ningxia Coal Industry Co.,Ltd.,Coal to Oil Branch,Yinchuan 750411,China), AuthorCompanyExt(id=1324788953156559046, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1324788948941283499, companyId=1324788953139781828, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=2国家能源集团 宁夏煤业有限责任公司 煤制油分公司,银川 750411)])])]
苏国庆1 , 李彦1, 张建文1 , 张志军2
作者信息
  • 1北京化工大学 机电工程学院,北京 100029
  • 2国家能源集团 宁夏煤业有限责任公司 煤制油分公司,银川 750411
通讯作者:
张建文(1969),男,教授,主要研究领域为化学工程、新/非常规能源技术与装备及化工安全等,通信地址:100029 北京市朝阳区北三环东路15号北京化工大学机电工程学院,E-mail:。
作者简介:

苏国庆(1994),男,主要研究方向为多相流腐蚀,通信地址:100029北京市朝阳区北三环东路15号北京化工大学机电工程学院,E-mail:。

Analysis of corrosion and leakage causes in heat exchangers of low‑temperature methanol washing units
Guoqing SU1 , Yan LI1, Jianwen ZHANG1 , Zhijun ZHANG2
Affiliations
  • 1College of Mechanical and Electrical Engineering,Beijing University of Chemical Technology,Beijing 100029,China
  • 2National Energy Group Ningxia Coal Industry Co.,Ltd.,Coal to Oil Branch,Yinchuan 750411,China
出版时间: 2025-03-30 doi: 10.3969/j.issn.1001-4837.2025.03.009
文章导航
收藏切换

为分析低温甲醇洗装置换热器的腐蚀泄漏原因,利用扫描电镜(SEM)、能谱仪(EDS)和X射线衍射仪(XRD),分别测定了失效管束的微观结构、元素分布和物相组成;利用X射线荧光光谱仪(XRF)测定封头处污泥的元素含量。此外,通过腐蚀模拟试验表征了富硫甲醇对换热管材质的腐蚀特性。结果表明,失效换热管存在多处腐蚀穿孔,最大直径为2.5 mm,腐蚀穿孔壁面近似垂直,且在其周围区域未发现异常减薄;腐蚀产物主要为硫铁化合物,同时在污泥中检测出大量含硫成分;高温显著加剧换热管材料腐蚀,80 ℃时腐蚀速率达到0.138 mm/a;在换热器运行过程中,富硫甲醇中H2S部分解吸形成了H2S-H2O电化学腐蚀环境,导致换热管出现均匀减薄,而污泥附着引发的垢下腐蚀是换热管腐蚀穿孔的主要原因。采取添加缓蚀阻垢剂、升级换热器材质等措施,可降低换热器的腐蚀风险,延长设备的运行周期。研究结果可为低温甲醇洗装置的腐蚀防控及换热器选型提供理论依据和工程参考。

换热器  /  泄漏  /  腐蚀分析  /  H2S腐蚀  /  垢下腐蚀

To analyze the corrosion and leakage causes in heat exchangers of low‑temperature methanol washing unit,scanning electron microscopy (SEM),energy‑dispersive spectroscopy (EDS) and X‑ray diffraction (XRD) were used to examine the microstructure,elemental distribution,and phase composition of the failed tubes.X‑ray fluorescence (XRF) was employed to determine the elemental content of sludge in the header.Additionally,corrosion simulation experiments were conducted to characterize the corrosive effects of sulfur‑rich methanol on the heat exchanger material.Results showed that multiple corrosion perforations (maximum diameter:2.5 mm) existed in the failed tubes,with perforation walls nearly perpendicular and no abnormal thinning observed in surrounding areas.The corrosion products primarily consisted of iron‑sulfur compounds,and significant sulfur‑containing components were detected in the sludge.High temperature markedly accelerated material corrosion,with a corrosion rate reaching 0.138 mm/a at 80 ℃.During operation,partial desorption of H2S from sulfur‑rich methanol formed an H2S-H2O electrochemical corrosion environment,leading to uniform thinning of the tubes.Under‑deposit corrosion caused by sludge adhesion was identified as the primary cause of perforation.Measures such as adding corrosion and scale inhibitors and upgrading the heat exchanger material can mitigate corrosion risks and extend equipment service life.The research can provide theoretical basis and engineering reference for corrosion prevention and control of low‑temperature methanol washing unit and heat exchanger selection.

heat exchanger  /  leakage  /  corrosion analysis  /  H2S corrosion  /  under‑deposit corrosion
苏国庆, 李彦, 张建文, 张志军. 低温甲醇洗装置换热器腐蚀泄漏原因分析. 压力容器, 2025 , 42 (3) : 71 -78 . DOI: 10.3969/j.issn.1001-4837.2025.03.009
Guoqing SU, Yan LI, Jianwen ZHANG, Zhijun ZHANG. Analysis of corrosion and leakage causes in heat exchangers of low‑temperature methanol washing units[J]. Pressure Vessel Technology, 2025 , 42 (3) : 71 -78 . DOI: 10.3969/j.issn.1001-4837.2025.03.009
低温甲醇洗是一种高效的气体净化工艺[1]。该工艺利用甲醇溶剂在低温条件下(-70~-30 ℃)对酸性气体的吸收能力,脱除工艺气体中的H2S,CO2和COS等有害物质。低温甲醇洗装置具有净化能力强、选择性高、技术成熟和操作成本低等优点,因此,在煤化工、石油化工等领域应用日益广泛[2-3]。
一般情况下,低温甲醇洗装置由吸收塔与再生塔两部分组成。为实现能量的综合有效利用,低温、富硫甲醇在进入再生塔前需先进入贫/富甲醇换热器进行预热[4]。然而,换热器内的高温、高压及高浓度酸性气体环境会引发一系列腐蚀失效问题。某公司低温甲醇洗装置换热器在运行过程中出现了严重泄漏,检修时发现换热管外表面出现大面积、不规则凹坑腐蚀,其中,部分凹坑腐蚀穿透造成泄漏。通过微观组织、金相和腐蚀物电镜分析,确定H2S腐蚀与CO2腐蚀的协同作用是造成换热器泄漏的主要原因[5-10]。霍跃光等[11]分析了某煤制油公司低温甲醇洗系统贫/富甲醇换热器的腐蚀泄漏事故,认为H2S腐蚀和羰基化合物腐蚀是泄漏的主要原因。此外,变换工段触媒粉化、瓷球破碎及煤粉夹带使得变换气粉尘含量超标,导致冲刷磨损也在一定程度上加剧了换热管的腐蚀损伤。张红卫等[12]研究了某低温甲醇洗绕管式换热器的泄漏原因,通过分析工艺运行数据,发现换热器管程的温度低于冰点,导致原料气中的饱和水结冰并附着在列管内;随着运行周期延长,列管内逐渐出现冰堵,最终导致大范围破裂与泄漏。陈志明[13]研究了某低温甲醇洗装置热再生塔再沸器的泄漏问题,分析了该换热器腐蚀的原因,认为湿H2S环境下奥氏体不锈钢易发生应力腐蚀。
由上述可知,目前已有许多关于低温甲醇洗换热器腐蚀的文献报道,但多数研究仅围绕泄漏原因开展定性分析,而对换热器腐蚀分布特征及工艺介质腐蚀特性等定量分析涉及较少。文中以某煤化工企业低温甲醇洗装置贫/富甲醇换热器为研究对象,通过管束失效分析、污泥成分分析及腐蚀模拟试验,深入探究换热器的腐蚀泄漏原因,并从设计制造和工艺操作方面提出腐蚀控制措施,为该类换热器的安全平稳运行提供理论支持。
图1示出低温甲醇洗装置的工艺流程。原料气在吸收塔中与贫硫甲醇逆流接触,脱除酸性气体。净化气从塔顶流出,随后被送往后续工序。富硫甲醇在进入再生塔之前,需先进入贫富甲醇换热器回收热量。通过高温汽提,富硫甲醇中的酸性气体在再生塔中完成解吸,并被送往硫回收装置;贫硫甲醇返回吸收塔,重新参与循环。
发生腐蚀泄漏的贫硫甲醇换热器的工艺参数和设备参数分别如表1、表2所示。根据现场调研结果,换热器的主要工艺参数均在设计指标范围内。富硫甲醇中水含量在0.8%左右;由于缺少合适的分析方法,富硫甲醇中的实际硫含量无法测定,但根据原料煤的硫含量数据(原料煤设计硫含量<1.8%,实际为0.6%~0.8%),可推算富硫甲醇中硫含量约为0.24%,该硫含量同样在设计指标范围内。
图2示出高压水冲洗前换热器不同部位的宏观腐蚀形貌。可以看出,换热器进口封头处出现轻微腐蚀,表面较为粗糙;出口封头处污泥呈黑色胶泥状,且只分布在出口封头,在取样过程中,发现污泥表现出很高的黏附性,同时散发强烈的刺鼻气味;管板腐蚀十分严重,表面附着有大面积黑色和棕黄色的腐蚀产物。
为深入探究换热器腐蚀泄漏的原因,充分冲洗换热器后,抽取一根泄漏严重的换热管进行后续试验,实物如图3所示。
由图3(a)可看出,失效换热管外壁呈红褐色,表面相对均匀、光滑。在管表面可观察到3处明显的腐蚀穿孔,孔洞直径分别为1.1,0.4,2.5 mm。根据装置运行数据,换热器在服役18个月后开始出现泄漏。结合换热管初始壁厚2.5 mm进行计算,得出服役期间管壁最大局部腐蚀速率约1.67 mm/a。使用超声波测厚仪测量换热管的厚度,结果表明,换热管整体有轻微减薄,减薄量约0.3 mm。同时,在腐蚀穿孔的周围区域未检测到异常减薄。
进一步沿轴向方向对换热管进行切割,其内表面如图3(b)所示。可以看出,换热管内壁有少量黑色和黄褐色腐蚀产物堆积。值得注意的是,所有腐蚀穿孔的壁面都近似垂直,不存在流体冲刷的痕迹。此外,在管内壁观察到多个尚未完全穿透壁面的腐蚀凹坑,这表明造成换热管失效泄漏的是管内介质,即富硫甲醇。
为观察换热管腐蚀表面的微观形貌,利用扫描电子显微镜(SEM)对样品内壁进行表征。该SEM设备型号Hitachi S4700,放大倍数为100倍,结果如图4所示。可以看出,样品表面覆盖着一层不均匀的腐蚀产物膜,且产物膜表面十分粗糙,结构完整性较差,局部区域分布有明显的沟壑。显然,这种结构的产物膜难以为基体提供充分的保护作用。流体会不断将腐蚀产物剥离壁面,加剧换热管的腐蚀损伤程度。此外,在样品表面还发现了大量裂纹。这些裂纹会削弱产物膜的完整性和致密性,进一步降低其对基体的保护作用。
采用能谱仪(EDS)测量样品内壁腐蚀表面的元素分布(测量位置见图4),结果见表3。可以看出,腐蚀表面元素有Fe,S,C,O四种,其中,Fe和S主要来自失效换热管的腐蚀产物,C和O主要来自取样/制样过程中金属的氧化及腐蚀表面残留的有机化合物。根据能谱分析结果,富硫甲醇中含有的H2S是导致换热器腐蚀泄漏的重要因素。
为分析腐蚀产物的物相组成,采用X射线衍射仪(XRD)对样品内壁进行表征。该XRD设备型号为Shimadzu 6000,扫描范围为10°~90°,结果如图5所示。可以看出,换热管内壁腐蚀产物的主要物相组成是3种硫铁化合物(FeS,FeS2,Fe3O4)。这表明在运行工况下,富硫甲醇中的H2S对换热管材料具有较强的腐蚀作用,二者之间发生了复杂的电化学腐蚀反应。
为进一步分析换热器腐蚀泄漏的原因,利用X射线荧光光谱仪(XRF)对封头处污泥进行元素含量测定。测定工作共分为2步:(1)对原始污泥样品进行测定;(2)对污泥样品进行800 ℃焚烧处理,研磨成粉末后进行第二次测定,处理过程如图6所示。XRF的设备型号为RIGAKU ZSX Primus,测量结果如表4所示。
可以看出,污泥样品中含有大量含硫成分。由于污泥具有很强的黏附性,因此,在换热器运行过程中极易黏附于换热管内壁,引发严重的垢下腐蚀。若长期积累,将导致换热管出现局部穿孔泄漏。
为探究富硫甲醇对换热管材料的腐蚀效果,参照GB 10124—1988《金属材料实验室均匀腐蚀全浸试验方法》,设计并开展腐蚀模拟试验。试样材料为10钢,尺寸为50 mm×20 mm×2 mm;试验温度分别为20,40,60,80 ℃。在换热器实际工况下,管程介质主要为液态富硫甲醇。文献[14-17]表明,在液相环境下,压力变化对腐蚀速率影响不明显,因此,试验过程中压力设定为常压。试验周期为12天,期间每隔4天更换新鲜试验溶液。为提高结果的可靠性,所有试验溶液均取自装置现场。试验结束后,使用扫描电镜观察试样的微观形貌,并称重计算平均腐蚀速率。
图7示出试样的微观腐蚀形貌。可以看出,当试验温度较低时,试样表面的腐蚀损伤较轻。随着温度进一步升高,试样的损伤程度呈加剧趋势。当温度为80 ℃时,试样表面十分粗糙,腐蚀产物膜出现严重破损,甚至在局部区域出现脱落。
图8示出不同温度下试样的平均腐蚀速率。
可以看出,温度变化对10钢的平均腐蚀速率具有明显影响。20 ℃下试样的平均腐蚀速率仅为0.019 mm/a,而80 ℃时腐蚀速率达到0.138 mm/a,两者相差超过7倍。由此可知,温度的升高显著削弱了10钢在富硫甲醇环境中的耐腐蚀性能。根据装置运行数据,换热器服役时长为2年,换热管壁厚均匀减薄了0.3 mm,试验数据与实际运行情况基本一致。
根据装置运行数据,富硫甲醇中所含CO2浓度极低。而且,在失效换热管表面和污泥样品中均未发现含碳腐蚀产物。综合各项分析,可以确定H2S腐蚀是换热器腐蚀泄漏的重要原因。根据生产工艺,在富硫甲醇从吸收塔流往解吸塔的过程中,其作为冷介质不断被加热,温度也从-36 ℃提升到了87 ℃。这就导致富硫甲醇中高浓度的H2S在换热器中发生了部分解吸。同时,前文已提及,富硫甲醇中含有少量液相水,因此换热器内部为典型的H2S-H2O电化学腐蚀环境。
一般情况下,H2S气体不会对金属产生腐蚀破坏作用。然而,当H2S溶解在液态水中时,会发生电离,并对10钢等低合金钢具有强腐蚀性[18]。H2S的电离反应如下:
H2S(aq)→k1H+(aq)+HS-(aq)
HS-(aq)→k2H+(aq)+S2-(aq)
式中,k1,k2为电离平衡常数,二者均为温度的函数。
环境温度越高,H2S的电离程度越高,电化学腐蚀反应速率越快。
电化学腐蚀的阳极反应方程如下:
Fe→Fe2++2e-
Fe2++S2-→FeS
Fe2++HS-→FeS+H+
电化学腐蚀的阴极反应方程[14]如下:
H++2e-→H2
碳钢设备的内壁表面除金属Fe外,还有部分氧化腐蚀产物,其主要成分为Fe2O3,Fe3O4及Fe(OH)3等。它们在缺氧环境下,可与湿H2S发生化学反应生成FeS[19],反应方程如下:
Fe2O3+3H2S→2FeS+3H2O+S
Fe3O4+4H2S→3FeS+4H2O+S
2FeOH3+3H2S→2FeS+6H2O+S
当环境温度超过50 ℃时,生成的FeS会与S进一步反应生成多硫化铁,反应方程如下:
FeS+S→FeS2
3FeS+S→Fe3S4
上述电化学腐蚀反应导致换热管壁厚均匀减薄。随着累积腐蚀时间的延长,换热管壁厚持续整体减薄,但不会出现大范围的腐蚀穿孔现象。针对管束的失效分析显示,腐蚀穿孔周围区域既无异常的厚度减薄,也无明显的冲刷痕迹,且所有腐蚀穿孔的壁面都近似垂直。结合现场调研和污泥分析结果,可判断污泥附着壁面造成的垢下腐蚀是换热管腐蚀穿孔的主要原因[20]。
图9示出换热管垢下腐蚀的机理。当管内局部流速较低时,来自上游装置的污泥黏附在壁表面,并逐渐沉积下来。随后,在污泥与管壁的交界处,会发生式(1)~(6)所示的电化学腐蚀反应,并形成垢下蚀坑。虽然污泥垢层隔绝了本体溶液,但由于其内部多孔结构提供了扩散通道,外界富硫甲醇中的H₂S仍能持续传递至垢层下方。同时,在闭塞区内,碳钢基体溶解产生的Fe²⁺会水解生成大量H⁺,导致电解质显著酸化[21]。此外,由于碳钢基体的电位明显低于腐蚀产物,其作为电偶腐蚀的阳极,腐蚀速率不断加快。可以看出,垢下腐蚀过程综合了点蚀、缝隙腐蚀和电偶腐蚀,具有典型的自催化特性。随着装置运行时间的延长,垢下蚀坑迅速加深,直至完全穿透换热管壁面,最终导致换热器泄漏失效[22-23]。
由于换热器管板不具备污泥沉积的条件,因此,其腐蚀类型以电化学腐蚀为主。腐蚀过程主要表现为管壁均匀减薄,管板表面粗糙且有大量腐蚀产物附着〔见图2(c)〕。此外,考虑到管板厚度较厚(20 mm),故在实际运行过程中发生失效泄漏的可能性较低。
(1)换热器的腐蚀主要集中在管程富硫甲醇一侧,同时在出口封头发现了大量具有刺激性气味的黏性污泥。
(2)失效换热管表面存在多处腐蚀穿孔,其最大直径为2.5 mm,腐蚀穿孔的周围区域未发现管壁异常减薄。腐蚀表面结构疏松且分布有大量裂纹,腐蚀产物的主要物相组成为FeS,FeS2和Fe3S4。此外,在污泥样品中发现了大量含硫成分。
(3)温度升高会显著削弱10钢在富硫甲醇中的耐蚀性能,80 ℃时腐蚀速率达到0.138 mm/a。
(4)在运行工况下,富硫甲醇中的H2S会在换热器中发生部分解吸,由此形成的H2S-H2O电化学腐蚀环境是换热器腐蚀的主要原因。污泥附着壁面造成的垢下腐蚀是换热管腐蚀穿孔的主要原因。
(1)加强对换热器工艺温度的控制。腐蚀模拟试验证实,温度的升高对材料平均腐蚀速率有显著影响。在实际运行过程中,应严格控制换热器进料温度,避免其长期高于设计值,从而确保换热器的整体腐蚀风险可防、可控。
(2)添加缓蚀阻垢剂。建议加入适量的缓蚀阻垢剂,不仅可减缓换热器的均匀腐蚀,还可减少污泥在管壁的黏附沉积,降低换热管发生垢下腐蚀穿孔的风险。此外,建议在换热器管程增设过滤设备,减少进入换热管的污泥量。
(3)升级换热器材质。对于H2S电化学腐蚀而言,奥氏体不锈钢具有优良的耐受性能[18]。因此,将换热器材质升级为304不锈钢,可大幅延长设备的运行周期。
  • 国家重点研发计划项目(2021YFB3301100);北京化工大学交叉学科项目(XK2023-07)
参考文献 引证文献
排序方式:
1
赖宁,于杰,魏成,等.低温甲醇洗装置运行问题及对策[J].化学工程,2022,50(11):74-78.
LAI N,YU J,WEI C,et al.Problems and counter measures of rectisol plant during operation[J].Chemical Engineering (China),2022,50(11):74-78.
2
王伟,杜丽.低温甲醇洗装置贫甲醇换热器换热管失效分析[J].化学工程与装备,2021(10):181-185.
WANG W,DU L.Failure analysis of lean methanol heat exchanger tube in the low‑temperature methanol wash unit[J].Chemical Engineering & Equipment,2021(10):181-185.
3
刘霞,何鹏.低温甲醇洗装置腐蚀分析与处理[J].山东化工,2021,50(1):125-126.
LIU X,HE P.Corrosion analysis and treatment of low‑temperature methanol washing unit[J].Shandong Chemical Industry,2021,50(1):125-126.
4
王克华,管凤宝,夏祖虎,等.煤制氢低温甲醇洗装置改造方案研究[J].现代化工,2023,43(11):231-235.
WANG K H,GUAN F B,XIA Z H,et al.Research on upgrading scheme for rectisol unit in a coal to hydrogen plant[J].Modern Chemical Industry,2023,43(11):231-235.
5
杨德忠,张坤,周明.低温甲醇洗甲醇换热器腐蚀原因分析[J].化工管理,2022(14):118-121.
YANG D Z,ZHANG K,ZHOU M.Analysis of corrosion causes of methanol heat exchanger[J].Chemical Engineering Management,2022(14):118-121.
6
苏国庆,李彦,窦站,等.硫回收装置余热锅炉铵盐结晶腐蚀机理研究[J].压力容器,2024,41(6):73-82.
SU G Q,LI Y,DOU Z,et al.Study on the corrosion mechanism of ammonium salt crystallization in waste heat boiler of a sulphur recovery unit[J].Pressure Vessel Technology,2024,41(6):73-82.
7
陈聚凯,吴肖文,周慧,等.基于CFD-DPM模拟的冷氢化工艺旋风分离器内气固两相流动及冲蚀磨损特性研究[J].流体机械,2024,52(10):41-48.
CHEN J K,WU X W,ZHOU H,et al.Study on characteristics of gas‑particle two‑phase flow and erosion in a cyclone separator used in cold hydrogenation process based on CFD-DPM modeling[J].Fluid Machinery,2024,52(10):41-48.
8
金浩哲,陈凤官,王超,等.煤气化装置黑水阀冲蚀磨损机理及智能防控研究[J].流体机械,2023,51(10):10-17.
JIN H Z,CHEN F G,WANG C,et al.Research on erosion wear mechanism and intelligent prevention and control of the black water valve in coal gasification plant[J].Fluid Machinery,2023,51(10):10-17.
9
刘忠伟,苗超,何萌,等.催化裂化提升管T型出口气固两相流冲蚀研究[J].流体机械,2024,52(10):74-81.
LIU Z W,MIAO C,HE M,et al.Study on erosion of gas-solid two‑phase flow at T‑type outlet of FCC riser[J].Fluid Machinery,2024,52(10):74-81.
10
葛伟伟,李庆昕,赵鑫鑫,等.陶瓷强化涂层在饮料灌装机中的应用[J].包装与食品机械,2023,41(5):46-51.
GE W W,LI Q X,ZHAO X X,et al.Application of ceramic strengthening coating in beverage filling machine[J].Packaging and Food Machinery,2023,41(5):46-51.
11
霍跃光,赵小波,邓金泉.低温甲醇洗系统贫富甲醇换热器泄漏原因分析及处理[J].煤化工,2020,48(1):64-66.
HUO Y G,ZHAO X B,DENG J Q.Analysis and treatment of leakage of lean‑rich methanol heat exchanger for the low‑temperature methanol washing system[J].Coal Chemical Industry,2020,48(1): 64-66.
12
张红卫,张武.低温甲醇洗绕管式换热器泄漏原因及处理措施[J].宁夏工程技术,2022,21(1):67-69.
ZHUANG H W,ZHANG W.Analysis of leakage causes and solutions of the cleaning of spiral wound heat exchanger in rectisol unit[J].Ningxia Engineering Technology,2022,21(1):67-69.
13
陈志明.低温甲醇洗换热器腐蚀问题浅析[J].内蒙古石油化工,2017,43(9):52-53.
CHEN Z M.A brief analysis of the corrosion issues in low‑temperature methanol wash heat exchangers[J].Inner Mongolia Petrochemical Industry,2017,43(9):52-53.
14
张玉福.多介质环境下压力容器用材腐蚀失效机理研究[D].兰州:兰州理工大学,2016.
ZHANG Y F.The research on the corrosion failure mechanism of pressure vessel materials under multi‑media environment[D].Lanzhou:Lanzhou University of Technology,2016.
15
冯桓榰,邢希金,谷林,等.高温高压高含硫气井T95技术套管腐蚀实验研究[J].表面技术,2018,47(12):21-29.
FENG H Z,XING X J,GU L,et al.Corrosion behavior of T95 casing in high temperature,high pressure and high H2S condition[J].Surface Technology,2018,47(12):21-29.
16
胡兴民,朱天寿,张书成,等.靖边气田天然气脱硫装置腐蚀行为研究[J].天然气工业,2007(5):121-123.
HU X M,ZHU T S,ZHANG S C,et al.Corrosion performance study on natural gas desulfurization unit in the Jingbian gas field[J].Natural Gas Industry,2007(5):121-123.
17
李春福.油气开发过程中的CO2腐蚀机理及防护技术研究[D].成都:西南石油学院,2005.
LI C F.Research on CO2 corrosion mechanism and protection technology in oil and gas development process[D].Chengdu:Southwest Petroleum Institute,2005.
18
李慧心.高含H2S环境下低合金钢腐蚀产物演化及其对腐蚀行为的影响[D].北京:北京科技大学,2019.
LI H X.Formation and evolution of H2S corrosion products and the influence on corrosion mechanism under high H2S partial pressure[D].Beijing:Beijing University of Science and Technology,2019.
19
管晨羽,李燕,张述伟.某厂低温甲醇洗中杂质硫的影响及消除研究[J].化学工程,2020,48(9):14-19.
GUAN C Y,LI Y,ZHANG S W.Study on influence and elimination of sulfide impurities in chilled methanol wash process of a plant[J].Chemical Engineering (China),2020,48(9):14-19.
20
贺三,罗斯琪,赵浩童,等.碳钢在CO2环境中无机垢下腐蚀研究进展[J].表面技术,2023,52(2):148-157.
HE S,LUO S Q,ZHAO H T,et al.Review of carbon steel under deposit corrosion in CO2 environment[J].Surface Technology,2023,52(2):148-157.
21
范金福,刘猛,张晓辰,等.流速对垢下腐蚀的影响及其腐蚀机理[J].腐蚀与防护,2019,40(11):810-815.
FAN J F,LIU M,ZHANG X C,et al.Effect of velocity on the under‑deposit corrosion and its corrosion mechanism[J].Corrosion & Protection,2019,40(11):810-815.
22
郭福平,吕运容,段志宏,等.重整装置双相不锈钢换热器腐蚀泄漏原因分析[J].压力容器,2023,40(4):59-66.
GUO F P,LYU Y R,DUAN Z H,et al.Analysis on corrosion leakage cause of duplex stainless steel heat exchanger in a catalytic reforming unit[J].Pressure Vessel Technology,2023,40(4):59-66.
23
蒋志国,王辉煌,龚利华,等.Cl-和H2S对不锈钢电化学行为的协同影响[J].材料保护,2017,50(2):74-77.
JIANG Z G,WANG H H,GONG L H,et al.Combined effects of Cl- and H2S on electrochemical behavior of stainless stee[J].Materials Protection,2017,50(2):74-77.
2025年第42卷第3期
134
63
0
引用本文
BibTeX
文章信息
doi: 10.3969/j.issn.1001-4837.2025.03.009
  • 接收时间:2025-01-19
  • 首发时间:2026-11-04
  • 出版时间:2025-03-30
补充材料
相关文章
文章信息
作者
出版历史
  • 收稿日期:2025-01-19
  • 修回日期:2025-02-28
基金
国家重点研发计划项目(2021YFB3301100);北京化工大学交叉学科项目(XK2023-07)
作者信息
    1北京化工大学 机电工程学院,北京 100029
    2国家能源集团 宁夏煤业有限责任公司 煤制油分公司,银川 750411

通讯作者:

张建文(1969),男,教授,主要研究领域为化学工程、新/非常规能源技术与装备及化工安全等,通信地址:100029 北京市朝阳区北三环东路15号北京化工大学机电工程学院,E-mail:。
参考文献
分享链接
https://castjournals.cast.org.cn/joweb/ylrq/CN/10.3969/j.issn.1001-4837.2025.03.009
分享至
全文二维码

扫描看全文

引用本文
BibTeX
本文的引用情况
2种不同金属材料的力学参数
科
Family
属数
Number of
genus
种数
Number of
species
占总种数比例
Percentage of
total species (%)
属
Genus
种数
Number of
species
占总种数比例
Percentage of total
species (%)
鹅膏菌科Amanitaceae 2 11 5.26 鹅膏菌属 Amanita 10 4.78
小菇科 Mycenaceae 2 12 5.74 丝盖伞属 Inocybe 5 2.39
多孔菌科 Polyporaceae 8 14 6.70 蜡蘑属 Laccaria 5 2.39
红菇科 Russulaceae 3 23 11.00 小皮伞属 Marasmius 6 2.87
小菇属 Mycena 11 5.26
光柄菇属 Pluteus 5 2.39
红菇属 Russula 17 8.13
栓菌属 Trametes 5 2.39
关闭全屏