Article(id=1327335687604515004, tenantId=1146029695717560320, journalId=1319355204128309394, issueId=1327335640930300759, articleNumber=null, orderNo=null, doi=10.3969/j.issn.1001-4837.2025.10.002, pmid=null, cstr=null, oa=null, hot=null, price=null, onlineType=0, articleFormat=0, articleType=null, articleTypeStr=null, receivedDate=1753459200000, receivedDateStr=2025-07-26, revisedDate=1758211200000, revisedDateStr=2025-09-19, acceptedDate=null, acceptedDateStr=null, onlineDate=1794391088629, onlineDateStr=2026-11-11, pubDate=1761753600000, pubDateStr=2025-10-30, doiRegisterDate=null, doiRegisterDateStr=null, onlineIssueDate=1794391088629, onlineIssueDateStr=2026-11-11, onlineJustAcceptDate=null, onlineJustAcceptDateStr=null, onlineFirstDate=null, onlineFirstDateStr=null, sourceXml=null, magXml=null, createTime=1794391088629, creator=13701087609, updateTime=1794391088629, updator=13701087609, issue=Issue{id=1327335640930300759, tenantId=1146029695717560320, journalId=1319355204128309394, year='2025', volume='42', issue='10', pageStart='1', pageEnd='86', issueExtLink='null', onlineDate='null', pubDate='1761753600000', pubDateStr='2025-10-30', beforeIssueId=null, nextIssueId=null, price=null, status=1, issueComplete=1, articleOrder=1, issueType=-1, specialIssue=null, createTime=1794391077500, creator='13701087609', updateTime=1794452618870, updator='13701087609', preIssue=null, nextIssue=null, articleTotal=null, ext={EN=IssueExt(id=1327593764446647258, tenantId=1146029695717560320, journalId=1319355204128309394, issueId=1327335640930300759, language=EN, specialIssueTitle=, coverIllustrator=null, specialIssueEditor=, specialIssueAbout=), CN=IssueExt(id=1327593764446647259, tenantId=1146029695717560320, journalId=1319355204128309394, issueId=1327335640930300759, language=CN, specialIssueTitle=, coverIllustrator=null, specialIssueEditor=, specialIssueAbout=)}, issueFiles=null, downloadFileDto=null}, startPage=23, endPage=30, ext={EN=ArticleExt(id=1327335688120414397, articleId=1327335687604515004, tenantId=1146029695717560320, journalId=1319355204128309394, language=EN, title=Study on the influence of interpass temperature on microstructure and properties of nickel‑based 690 welding wire deposited metal, columnId=1320422992476226524, journalTitle=Pressure Vessel Technology, columnName=Experimental Researches, runingTitle=null, highlight=null, articleAbstract=

To address the issue of inconsistent interpass temperatures during welding of nuclear island main equipment components,the TIG welding method was used to study the influence of interpass temperature on the microstructure evolution and mechanical properties of nickel‑based 690 welding wire deposited metal.Combined with mechanical property tests such as tensile and impact,as well as microstructural observations using OM,SEM and EDS,the results show that as the interpass temperature increases,the room‑temperature mechanical properties of the deposited metal improve insignificantly,but both strength and plasticity at 350 ℃ are enhanced.With increasing interpass temperature,the weld formation coefficient decreases,while the fluidity of the molten pool and weldability improve significantly,and the high‑temperature heat accumulation effect intensifies,promoting molten pool flow and grain boundary migration,thereby increasing the orientation regularity of columnar grains in the overlapping zone across weld passes.When the interpass temperature exceeds 225 ℃,microcracks are prone to form in the microstructure.SEM and EDS analyses reveal that these cracks exhibit step‑like propagation morphology,accompanied by O/Si element enrichment and Ti/Nb element segregation,consistent with the characteristics of ductility‑dip cracking(DDC).This study provides a reference for establishing reasonable interpass temperature processes in nuclear power equipment welding.

, authors=Wei FENG1, Han MENG1, 2, Xinghai HAN1, Bo CHEN1, Guofo WANG1, authorsList=Wei FENG, Han MENG, Xinghai HAN, Bo CHEN, Guofo WANG, authorCompany=null, correspAuthors=null, authorNote=null, correspAuthorsNote=null, copyrightStatement=null, copyrightOwner=null, extLink=null, articleAbsUrl=null, sourceXml=null, magXml=null, pdfUrl=null, pdf=null, pdfFileSize=null, pdfExtLink=null, richHtmlUrl=null, mobilePdfUrl=null, reviewReport=null, pdfFirstPage=null, abstractGraph=null, abstractGraphContent=null, abstractVideo=null, citation=null, cebUrl=null, magXmlContent=null, mapNumber=null, fund=null), CN=ArticleExt(id=1327335690888655065, articleId=1327335687604515004, tenantId=1146029695717560320, journalId=1319355204128309394, language=CN, title=道间温度对镍基690焊丝熔敷金属组织及性能影响研究, columnId=1320422992698524638, journalTitle=压力容器, columnName=试验研究, runingTitle=null, highlight=null, articleAbstract=

针对核岛主设备各装置焊接过程中道间温度不统一的问题,采用TIG焊方法研究道间温度对镍基690焊丝熔敷金属组织演变及力学性能的影响规律。结合拉伸、冲击等力学性能测试,以及OM,SEM,EDS等微观组织观察,结果表明:随道间温度升高,熔敷金属的室温力学性能提升不明显,但350 ℃下的强度和塑性均有所提升;随道间温度的升高,焊缝成形系数减小,熔池流动性及焊接工艺性显著改善,高温热累积效应增强,促进了熔池流动与晶界迁移,跨焊道搭接区柱状晶的取向规整度提高;当道间温度超过225 ℃时,金相组织易产生微裂纹,通过SEM,EDS分析发现,其表现为台阶状扩展形貌,并伴有O/Si元素富集及Ti/Nb元素偏析,符合高温低塑性裂纹(DDC)的特征。研究可为核电设备焊接制定合理的道间温度工艺提供参考。

, authors=冯伟1, 孟涵1, 2, 韩兴海1, 陈波1, 王国佛1, authorsList=冯伟, 孟涵, 韩兴海, 陈波, 王国佛, authorCompany=null, correspAuthors=null, authorNote=

冯伟(1981),男,正高级工程师,主要从事特种焊接材料研发工作,通信地址:150060黑龙江省哈尔滨市平房区渤海路21号哈尔滨威尔焊接有限责任公司,E-mail:。

, correspAuthorsNote=null, copyrightStatement=作者向本刊所投稿件一经本刊录用,则该论文的复制权、发行权、信息网络传播权、翻译权、汇编权等权利视为自动转让给本刊。本刊为国内各主要数据库收录期刊,本刊所发表的稿件将同时通过因特网进行网络出版或提供信息服务(包括印刷版、光盘版和网络版等各种使用方式)。, copyrightOwner=null, extLink=null, articleAbsUrl=null, sourceXml=/YPWtByZG4UA8maygLK7kg==, magXml=fBsi+nbaeyrQ5Y2yOaUrvg==, pdfUrl=null, pdf=m0zprspMqHU8Q+SJlJ7pFw==, pdfFileSize=8082598, pdfExtLink=null, richHtmlUrl=null, mobilePdfUrl=null, reviewReport=null, pdfFirstPage=null, abstractGraph=Lc9dApdDN0LUAbGVGCQ4bA==, abstractGraphContent=null, abstractVideo=null, citation=null, cebUrl=null, magXmlContent=luNJ9UKMlf7NuWYcNRksAw==, mapNumber=null, fund=null)}, authors=[Author(id=1327335691261948129, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, orderNo=0, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=Fengwei323412@163.com, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335691324862691, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335691261948129, language=EN, stringName=Wei FENG, firstName=Wei, middleName=null, lastName=FENG, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335691391971556, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335691261948129, language=CN, stringName=冯伟, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060, bio={"content":"

冯伟(1981),男,正高级工程师,主要从事特种焊接材料研发工作,通信地址:150060黑龙江省哈尔滨市平房区渤海路21号哈尔滨威尔焊接有限责任公司,E-mail:。

"}, bioImg=null, bioContent=

冯伟(1981),男,正高级工程师,主要从事特种焊接材料研发工作,通信地址:150060黑龙江省哈尔滨市平房区渤海路21号哈尔滨威尔焊接有限责任公司,E-mail:。

, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335691077398746, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, xref=1, ext=[AuthorCompanyExt(id=1327335691094175963, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China), AuthorCompanyExt(id=1327335691102564572, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060)])]), Author(id=1327335691450691814, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, orderNo=1, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335691551355113, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335691450691814, language=EN, stringName=Han MENG, firstName=Han, middleName=null, lastName=MENG, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, 2, address=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China
2Harbin Welding Institute Limited Company,Harbin 150028,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335691618463978, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335691450691814, language=CN, stringName=孟涵, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, 2, address=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060
2中国机械总院集团哈尔滨焊接研究所有限公司,哈尔滨 150028, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335691077398746, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, xref=1, ext=[AuthorCompanyExt(id=1327335691094175963, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China), AuthorCompanyExt(id=1327335691102564572, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060)]), AuthorCompany(id=1327335691161284829, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, xref=2, ext=[AuthorCompanyExt(id=1327335691182256350, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691161284829, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=2Harbin Welding Institute Limited Company,Harbin 150028,China), AuthorCompanyExt(id=1327335691190644959, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691161284829, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=2中国机械总院集团哈尔滨焊接研究所有限公司,哈尔滨 150028)])]), Author(id=1327335691681378540, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, orderNo=2, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335691752681710, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335691681378540, language=EN, stringName=Xinghai HAN, firstName=Xinghai, middleName=null, lastName=HAN, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335691832373487, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335691681378540, language=CN, stringName=韩兴海, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335691077398746, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, xref=1, ext=[AuthorCompanyExt(id=1327335691094175963, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China), AuthorCompanyExt(id=1327335691102564572, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060)])]), Author(id=1327335691912065265, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, orderNo=3, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335692004339955, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335691912065265, language=EN, stringName=Bo CHEN, firstName=Bo, middleName=null, lastName=CHEN, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335692105003252, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335691912065265, language=CN, stringName=陈波, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335691077398746, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, xref=1, ext=[AuthorCompanyExt(id=1327335691094175963, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China), AuthorCompanyExt(id=1327335691102564572, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060)])]), Author(id=1327335692167917814, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, orderNo=4, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335692289552632, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335692167917814, language=EN, stringName=Guofo WANG, firstName=Guofo, middleName=null, lastName=WANG, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335692360855801, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335692167917814, language=CN, stringName=王国佛, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335691077398746, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, xref=1, ext=[AuthorCompanyExt(id=1327335691094175963, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China), AuthorCompanyExt(id=1327335691102564572, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060)])])], keywords=[Keyword(id=1327335692469907706, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, orderNo=1, keyword=Inconel 690), Keyword(id=1327335692532822267, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, orderNo=2, keyword=hot cracking), Keyword(id=1327335692612514044, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, orderNo=3, keyword=interpass temperature), Keyword(id=1327335692696400125, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, orderNo=4, keyword=ductility‑dip cracking(DDC)), Keyword(id=1327335692759314686, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, orderNo=1, keyword=Inconel 690), Keyword(id=1327335692830617855, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, orderNo=2, keyword=热裂纹), Keyword(id=1327335692897726720, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, orderNo=3, keyword=道间温度), Keyword(id=1327335692956446977, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, orderNo=4, keyword=高温低塑性裂纹(DDC))], refs=[Reference(id=1327335695938597161, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, doi=null, pmid=null, pmcid=null, year=1979, volume=28, issue=2, pageStart=82, pageEnd=95, url=null, language=null, rfNumber=1, rfOrder=0, authorNames=SEDRIKS A J, SCHULTZ J W, CORDOVI M A, journalName=Corrosion Engineering, refType=null, unstructuredReference=SEDRIKS A J,SCHULTZ J W,CORDOVI M A.Inconel alloy 690-A new corrosion resistant material[J].Corrosion Engineering,1979,28(2):82-95., articleTitle=Inconel alloy 690-A new corrosion resistant material, refAbstract=null), Reference(id=1327335695997317418, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, doi=null, pmid=null, pmcid=null, year=2012, volume=null, issue=null, pageStart=1, pageEnd=15, url=null, language=null, rfNumber=2, rfOrder=1, authorNames=ZHANG R G, CARUSO M, KISER S, journalName=null, refType=null, unstructuredReference=ZHANG R G,CARUSO M,KISER S,et al.New 30% chromium‑containing Ni-Cr-Fe welding product provides outstanding resistance to PWSCC,ductility dip cracking (DDC) and meets all other nuclear welding requirements[C]//Corrosion 2012.Association for Materials Protection and Performance,2012:1-15., articleTitle=New 30% chromium‑containing Ni-Cr-Fe welding product provides outstanding resistance to PWSCC,ductility dip cracking (DDC) and meets all other nuclear welding requirements, refAbstract=null), Reference(id=1327335696068620587, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, doi=null, pmid=null, pmcid=null, year=2009, volume=null, issue=null, pageStart=null, pageEnd=null, url=null, language=null, rfNumber=3, rfOrder=2, authorNames=KISER S D, ZHANG R, BAKER B A, journalName=null, refType=null, unstructuredReference=KISER S D,ZHANG R,BAKER B A.A new welding material for improved resistance to ductility dip cracking[C]//International Conference on Trends in Welding Research.2009., articleTitle=A new welding material for improved resistance to ductility dip cracking, refAbstract=null), Reference(id=1327335696139923756, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, doi=null, pmid=null, pmcid=null, year=2016, volume=29, issue=10, pageStart=928, pageEnd=939, url=null, language=null, rfNumber=4, rfOrder=3, authorNames=ZHANG X, LI D Z, LI Y Y, journalName=Acta Metallurgica Sinica (English Letters), refType=null, unstructuredReference=ZHANG X,LI D Z,LI Y Y,et al.Effect of Nb and Mo on the microstructure, mechanical properties and ductility-dip cracking of Ni–Cr–Fe weld metals[J].Acta Metallurgica Sinica (English Letters),2016,29(10):928-939., articleTitle=Effect of Nb and Mo on the microstructure, mechanical properties and ductility-dip cracking of Ni–Cr–Fe weld metals, refAbstract=null), Reference(id=1327335696198644013, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, doi=null, pmid=null, pmcid=null, year=2015, volume=46, issue=null, pageStart=1227, pageEnd=1236, url=null, language=null, rfNumber=5, rfOrder=4, authorNames=QIN R Y, WANG H, HE G, journalName=Metallurgical and Materials Transactions A, refType=null, unstructuredReference=QIN R Y,WANG H,HE G.Investigation on the microstructure and ductility‑dip cracking susceptibility of the butt weld welded with ENiCrFe-7 nickel-base alloy‑covered electrodes[J].Metallurgical and Materials Transactions A,2015,46:1227-1236., articleTitle=Investigation on the microstructure and ductility‑dip cracking susceptibility of the butt weld welded with ENiCrFe-7 nickel-base alloy‑covered electrodes, refAbstract=null), Reference(id=1327335696265752878, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, doi=null, pmid=null, pmcid=null, year=2013, volume=29, issue=5, pageStart=458, pageEnd=466, url=null, language=null, rfNumber=6, rfOrder=5, authorNames=MO W L, LU S P, LI D Z, journalName=Journal of Materials Science & Technology, refType=null, unstructuredReference=MO W L,LU S P,LI D Z,et al.Effects of filler metal composition on inclusions and inclusion defects for ER NiCrFe-7 weldments[J].Journal of Materials Science & Technology,2013,29(5):458-466., articleTitle=Effects of filler metal composition on inclusions and inclusion defects for ER NiCrFe-7 weldments, refAbstract=null), Reference(id=1327335696341250351, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, doi=null, pmid=null, pmcid=null, year=2017, volume=null, issue=null, pageStart=null, pageEnd=null, url=null, language=null, rfNumber=7, rfOrder=6, authorNames=RAPETTI, A, TODESCHINI, P, HENDILI, S, journalName=Proceedings of the ASME 2017 Pressure Vessels and Piping Conference, refType=null, unstructuredReference=RAPETTI, A, TODESCHINI, P, HENDILI, S,et al.A Study of ductility dip cracking of inconel 690 welding filler metal:development of a refusion cracking test[J].Proceedings of the ASME 2017 Pressure Vessels and Piping Conference,2017:V06BT06A022., articleTitle=A Study of ductility dip cracking of inconel 690 welding filler metal:development of a refusion cracking test, refAbstract=null), Reference(id=1327335696408359216, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, doi=null, pmid=null, pmcid=null, year=2012, volume=null, issue=9, pageStart=31, pageEnd=36, url=null, language=null, rfNumber=8, rfOrder=7, authorNames=霍树斌, 陈佩寅, 陈燕, journalName=焊接, refType=null, unstructuredReference=霍树斌,陈佩寅,陈燕,等.核用Inconel 690焊丝TIG焊微裂纹产生机理研究[J].焊接,2012(9):31-36., articleTitle=核用Inconel 690焊丝TIG焊微裂纹产生机理研究, refAbstract=null), Reference(id=1327335696467079473, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, doi=null, pmid=null, pmcid=null, year=2012, volume=null, issue=9, pageStart=31, pageEnd=36, url=null, language=null, rfNumber=8, rfOrder=8, authorNames=HUO S B, CHEN P Y, CHEN Y, journalName=Welding & Joining, refType=null, unstructuredReference=HUO S B,CHEN P Y,CHEN Y,et.al.Mechanism study on micro‑crack formation in tig welds using nuclear-grade inconel 690 filler wire[J].Welding & Joining,2012(9):31-36., articleTitle=Mechanism study on micro‑crack formation in tig welds using nuclear-grade inconel 690 filler wire, refAbstract=null), Reference(id=1327335696567742770, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, doi=null, pmid=null, pmcid=null, year=2016, volume=60, issue=5, pageStart=951, pageEnd=961, url=null, language=null, rfNumber=9, rfOrder=9, authorNames=FINK C, ZINKE M, JÜTTNER S, journalName=Welding in the World, refType=null, unstructuredReference=FINK C,ZINKE M,JÜTTNER S.An investigation of ductility‑dip cracking in the base metal heat‑affected zone of wrought nickel base alloys—Part Ⅱ:Correlation of PVR and STF results[J].Welding in the World,2016,60(5):951-961., articleTitle=An investigation of ductility‑dip cracking in the base metal heat‑affected zone of wrought nickel base alloys—Part Ⅱ:Correlation of PVR and STF results, refAbstract=null), Reference(id=1327335696626463027, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, doi=null, pmid=null, pmcid=null, year=2016, volume=60, issue=5, pageStart=939, pageEnd=950, url=null, language=null, rfNumber=10, rfOrder=10, authorNames=FINK C, journalName=Welding in the World, refType=null, unstructuredReference=FINK C.An investigation on ductility‑dip cracking in the base metal heat‑affected zone of wrought nickel base alloys—Part Ⅰ:Metallurgical effects and cracking mechanism[J].Welding in the World,2016,60(5):939-950., articleTitle=An investigation on ductility‑dip cracking in the base metal heat‑affected zone of wrought nickel base alloys—Part Ⅰ:Metallurgical effects and cracking mechanism, refAbstract=null), Reference(id=1327335696697766196, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, doi=null, pmid=null, pmcid=null, year=2017, volume=61, issue=6, pageStart=1155, pageEnd=1168, url=null, language=null, rfNumber=11, rfOrder=11, authorNames=WANG X L, TSAI Y T, YANG J R, journalName=Welding in the World, refType=null, unstructuredReference=WANG X L,TSAI Y T,YANG J R,et al.Effect of interpass temperature on the microstructure and mechanical properties of multi‑pass weld metal in a 550‑MPa‑grade offshore engineering steel[J].Welding in the World,2017,61(6):1155-1168., articleTitle=Effect of interpass temperature on the microstructure and mechanical properties of multi‑pass weld metal in a 550‑MPa‑grade offshore engineering steel, refAbstract=null), Reference(id=1327335696773263670, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, doi=null, pmid=null, pmcid=null, year=2011, volume=null, issue=null, pageStart=null, pageEnd=null, url=null, language=null, rfNumber=12, rfOrder=12, authorNames=PETRO J S, journalName=null, refType=null, unstructuredReference=PETRO J S.Effect of interpass temperature on the structure and properties of multipass weldments in high performance nickel alloys[D].Colorado:Colorado State University,2011., articleTitle=Effect of interpass temperature on the structure and properties of multipass weldments in high performance nickel alloys, refAbstract=null), Reference(id=1327335696848761143, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, doi=null, pmid=null, pmcid=null, year=2007, volume=51, issue=9/10, pageStart=24, pageEnd=30, url=null, language=null, rfNumber=13, rfOrder=13, authorNames=LIPPOLD J C, NISSLEY N E, journalName=Welding in the World, refType=null, unstructuredReference=LIPPOLD J C,NISSLEY N E.Further investigations of ductility‑dip cracking in high chromium,Ni‑base filler metals[J].Welding in the World,2007,51(9/10):24-30., articleTitle=Further investigations of ductility‑dip cracking in high chromium,Ni‑base filler metals, refAbstract=null)], funds=null, companyList=[AuthorCompany(id=1327335691077398746, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, xref=1, ext=[AuthorCompanyExt(id=1327335691094175963, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China), AuthorCompanyExt(id=1327335691102564572, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060)]), AuthorCompany(id=1327335691161284829, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, xref=2, ext=[AuthorCompanyExt(id=1327335691182256350, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691161284829, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=2Harbin Welding Institute Limited Company,Harbin 150028,China), AuthorCompanyExt(id=1327335691190644959, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691161284829, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=2中国机械总院集团哈尔滨焊接研究所有限公司,哈尔滨 150028)])], figs=[ArticleFig(id=1327335693099053314, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, label=Fig.1, caption=Schematic of welded joint, figureFileSmall=wl4AkmUQy+5DzvyGY6pRag==, figureFileBig=Lc9dApdDN0LUAbGVGCQ4bA==, tableContent=null), ArticleFig(id=1327335693166162179, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, label=图1, caption=焊接接头示意, figureFileSmall=wl4AkmUQy+5DzvyGY6pRag==, figureFileBig=Lc9dApdDN0LUAbGVGCQ4bA==, tableContent=null), ArticleFig(id=1327335693338128644, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, label=Fig.2, caption=Room‑temperature mechanical properties of deposited metal under different interpass temperatures, figureFileSmall=oEC5Q6YTOBi8pT54q5ASCg==, figureFileBig=ZOluQmx2RdfnUqsrAwpy3A==, tableContent=null), ArticleFig(id=1327335693430403333, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, label=图2, caption=不同道间温度下熔敷金属室温力学性能, figureFileSmall=oEC5Q6YTOBi8pT54q5ASCg==, figureFileBig=ZOluQmx2RdfnUqsrAwpy3A==, tableContent=null), ArticleFig(id=1327335693522678022, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, label=Fig.3, caption=Mechanical properties of deposited metal at 350 ℃ under different interpass temperatures, figureFileSmall=ByrNIlMWPpzAcLO/N+RrEw==, figureFileBig=Lry1dTZ6Wiuj3+07cVRnxQ==, tableContent=null), ArticleFig(id=1327335693598175495, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, label=图3, caption=不同道间温度下熔敷金属在350 ℃时的力学性能, figureFileSmall=ByrNIlMWPpzAcLO/N+RrEw==, figureFileBig=Lry1dTZ6Wiuj3+07cVRnxQ==, tableContent=null), ArticleFig(id=1327335693669478664, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, label=Fig.4, caption=Cross‑sectional dimensions of single weld bead for WHS690M welding wire under different interpass temperatures, figureFileSmall=4SzsKCEsagfG1hfPyriDpQ==, figureFileBig=81UXrG1Xjp0Qss0bYzYa3g==, tableContent=null), ArticleFig(id=1327335693774336266, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, label=图4, caption=不同道间温度下WHS690M焊丝单焊道截面尺寸, figureFileSmall=4SzsKCEsagfG1hfPyriDpQ==, figureFileBig=81UXrG1Xjp0Qss0bYzYa3g==, tableContent=null), ArticleFig(id=1327335693841445131, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, label=Fig.5, caption=Reinforcement height,contact angle,penetration depth and bead width of single weld bead for WHS690M welding wire under different interpass temperatures, figureFileSmall=tPuFk0hp/aCwYsj+MLZtJQ==, figureFileBig=iGz5AtSf049rcdo1cEdtAQ==, tableContent=null), ArticleFig(id=1327335693958885644, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, label=图5, caption=不同道间温度下WHS690M焊丝单焊道余高、接触角、熔深及熔宽, figureFileSmall=tPuFk0hp/aCwYsj+MLZtJQ==, figureFileBig=iGz5AtSf049rcdo1cEdtAQ==, tableContent=null), ArticleFig(id=1327335694038577421, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, label=Fig.6, caption=Weld size and weld forming coefficient under different interpass temperatures, figureFileSmall=gxfg9bIfDaWtMQ36xzVBDA==, figureFileBig=Izpw6z29BaaF82XNVbIN2Q==, tableContent=null), ArticleFig(id=1327335694139240718, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, label=图6, caption=不同道间温度下焊道尺寸及焊缝成形系数, figureFileSmall=gxfg9bIfDaWtMQ36xzVBDA==, figureFileBig=Izpw6z29BaaF82XNVbIN2Q==, tableContent=null), ArticleFig(id=1327335694244098319, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, label=Fig.7, caption=Macroscopic morphology of deposited metal, figureFileSmall=jpL0V9LABK/Jpjb0TYARjg==, figureFileBig=JtN5tiFsY24a08zQQF5suQ==, tableContent=null), ArticleFig(id=1327335694319595792, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, label=图7, caption=熔敷金属宏观形貌, figureFileSmall=jpL0V9LABK/Jpjb0TYARjg==, figureFileBig=JtN5tiFsY24a08zQQF5suQ==, tableContent=null), ArticleFig(id=1327335694407676177, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, label=Fig.8, caption=Microstructure of overlap region of deposited metal, figureFileSmall=sh/1PEbIQwbX5gt+XDUeQg==, figureFileBig=9h7Na2JS46vzyVw/C1QjkQ==, tableContent=null), ArticleFig(id=1327335694474785042, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, label=图8, caption=熔敷金属搭接处金相组织, figureFileSmall=sh/1PEbIQwbX5gt+XDUeQg==, figureFileBig=9h7Na2JS46vzyVw/C1QjkQ==, tableContent=null), ArticleFig(id=1327335694546088211, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, label=Fig.9, caption=Microstructure of cracks within interpass temperature range of 225~275 ℃, figureFileSmall=4j4s15QCwpAdn2FybqOnTg==, figureFileBig=9SmXhrDuDXtGcOZRcSNsBw==, tableContent=null), ArticleFig(id=1327335694629974292, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, label=图9, caption=道间温度225~275 ℃范围内裂纹金相组织, figureFileSmall=4j4s15QCwpAdn2FybqOnTg==, figureFileBig=9SmXhrDuDXtGcOZRcSNsBw==, tableContent=null), ArticleFig(id=1327335694701277461, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, label=Fig.10, caption=Schematic of functional relationship between temperature and ductility for welding crack occurrence in nickel‑based alloys, figureFileSmall=gwZ+F6JE0Ye2zbg5YHvSfw==, figureFileBig=T0Jzoka/VGp66b2lDd71vw==, tableContent=null), ArticleFig(id=1327335694764192022, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, label=图10, caption=镍基合金中焊接裂纹发生的温度与延性函数关系示意, figureFileSmall=gwZ+F6JE0Ye2zbg5YHvSfw==, figureFileBig=T0Jzoka/VGp66b2lDd71vw==, tableContent=null), ArticleFig(id=1327335694831300887, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, label=Fig.11, caption=SEM images of crack fracture surface within interpass temperature range of 225~275 ℃, figureFileSmall=eylawUQD2/dbfd5ZCeWxGg==, figureFileBig=ePHXNdFVDTGjOi39BzeC6w==, tableContent=null), ArticleFig(id=1327335694898409752, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, label=图11, caption=道间温度225~275 ℃范围内裂纹断口SEM图, figureFileSmall=eylawUQD2/dbfd5ZCeWxGg==, figureFileBig=ePHXNdFVDTGjOi39BzeC6w==, tableContent=null), ArticleFig(id=1327335694965518617, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, label=Fig.12, caption=SEM images of step region on crack fracture surface within interpass temperature range of 225~275 ℃, figureFileSmall=EmAUtZWS0nT1Ng42lP0dCA==, figureFileBig=+Oa6kkIonI9YuCI3RXAT6g==, tableContent=null), ArticleFig(id=1327335695028433178, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, label=图12, caption=道间温度225~275 ℃范围内裂纹断口台阶区SEM图, figureFileSmall=EmAUtZWS0nT1Ng42lP0dCA==, figureFileBig=+Oa6kkIonI9YuCI3RXAT6g==, tableContent=null), ArticleFig(id=1327335695082959131, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, label=Fig.13, caption=EDS analysis region of crack fracture surface within interpass temperature range of 225~275 ℃, figureFileSmall=1bLtKIQ0OMgdB1PYqwfgBQ==, figureFileBig=KSDZSVB8RvYpnQL3OaQ5Iw==, tableContent=null), ArticleFig(id=1327335695141679389, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, label=图13, caption=道间温度225~275 ℃内EDS裂纹断口分析区域, figureFileSmall=1bLtKIQ0OMgdB1PYqwfgBQ==, figureFileBig=KSDZSVB8RvYpnQL3OaQ5Iw==, tableContent=null), ArticleFig(id=1327335695204593950, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, label=Tab.1, caption=

Chemical composition of WHS690M welding wire

, figureFileSmall=null, figureFileBig=null, tableContent=
元素CSiMnAlTiCrNiFeNb+Ta
含量0.020.210.720.200.5429.1858.409.770.85
), ArticleFig(id=1327335695292674335, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, label=表1, caption=

WHS690M焊丝化学成分

, figureFileSmall=null, figureFileBig=null, tableContent=
元素CSiMnAlTiCrNiFeNb+Ta
含量0.020.210.720.200.5429.1858.409.770.85
), ArticleFig(id=1327335695363977504, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, label=Tab.2, caption=

Welding process parameters

, figureFileSmall=null, figureFileBig=null, tableContent=
参数焊接电流/A电弧电压/V焊接速度/(mm·min-1)氩气流量/(L·min-1)
数值2301511025
), ArticleFig(id=1327335695431086369, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, label=表2, caption=

焊接工艺参数

, figureFileSmall=null, figureFileBig=null, tableContent=
参数焊接电流/A电弧电压/V焊接速度/(mm·min-1)氩气流量/(L·min-1)
数值2301511025
), ArticleFig(id=1327335695502389538, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, label=Tab.3, caption=

Mechanical properties of the deposited metal at room temperature and 350 ℃ under different interpass temperatures

, figureFileSmall=null, figureFileBig=null, tableContent=
道间温度/℃试验温度抗拉强度/MPa屈服强度/MPa断面收缩率/%断后伸长率/%
75~121室温6194034659
350 ℃50033339.553
121~177室温6063984263
350 ℃4973414059
177~225室温6254124761
350 ℃50332145.558
225~275室温6193964263
350 ℃5093104762
), ArticleFig(id=1327335695577887012, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, label=表3, caption=

不同道间温度下熔敷金属在室温及350 ℃时的力学性能

, figureFileSmall=null, figureFileBig=null, tableContent=
道间温度/℃试验温度抗拉强度/MPa屈服强度/MPa断面收缩率/%断后伸长率/%
75~121室温6194034659
350 ℃50033339.553
121~177室温6063984263
350 ℃4973414059
177~225室温6254124761
350 ℃50332145.558
225~275室温6193964263
350 ℃5093104762
), ArticleFig(id=1327335695644995877, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, label=Tab.4, caption=

Room‑temperature impact test and bending test results of deposited metal

, figureFileSmall=null, figureFileBig=null, tableContent=
道间温度/℃冲击吸收能量KV2/J180°侧向弯曲试验(D=4a)
75~121249.0,201.5,242.0无裂纹
121~177213.2,200.0,200.0无裂纹
177~225233.6,209.5,205.9无裂纹
225~275236.4,239.8,221.2无裂纹
), ArticleFig(id=1327335695703716134, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, label=表4, caption=

熔敷金属室温冲击试验及弯曲试验结果

, figureFileSmall=null, figureFileBig=null, tableContent=
道间温度/℃冲击吸收能量KV2/J180°侧向弯曲试验(D=4a)
75~121249.0,201.5,242.0无裂纹
121~177213.2,200.0,200.0无裂纹
177~225233.6,209.5,205.9无裂纹
225~275236.4,239.8,221.2无裂纹
), ArticleFig(id=1327335695775019303, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=EN, label=Tab.5, caption=

EDS analysis results within interpass temperature range of 225~275 ℃

, figureFileSmall=null, figureFileBig=null, tableContent=
元素OAlSiTiMnNb
谱图61.970.240.431.110.881.70
谱图72.58—1.320.740.820.95
), ArticleFig(id=1327335695846322472, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, language=CN, label=表5, caption=

道间温度225~275 ℃范围内EDS分析结果

, figureFileSmall=null, figureFileBig=null, tableContent=
元素OAlSiTiMnNb
谱图61.970.240.431.110.881.70
谱图72.58—1.320.740.820.95
)], attaches=null, journal=Journal(id=1319354845020389520, delFlag=0, nameCn=压力容器, nameEn=Pressure Vessel Technology, nameHistory1=null, nameHistory2=null, issn=1001-4837, eissn=null, cn=34-1058/TH, coden=null, periodic=0, language=CN, oaType=null, ccby=null, superviseOffice=null, ownerOffice=null, pubOffice=null, editorOffice=null, officeType=null, aims=null, clcCode=null, officeProv=null, officeCity=null, officeAddr=null, officeZip=null, officeEmail=null, officePhone=null, editDirector=null, officeDirector=null, officeDirectorPhone=null, officeStaffNum=null, officeEmpNum=null, coverPicUrl=jxjNdnQvHSQ8b9q0zS7Bgw==, journalPrice=null, startedYear=null, abbrevIsoEn=Pressure Vessel Technology, journalRemark=null, publicationField=null, createdTime=1792488307482, updatedTime=1792488496537, createdBy=18614031015, updatedBy=13701087609, firstLetterCn=Y, firstLetterEn=Y, subjectCode=Engineering, subjectName=null, subjectCodeEn=Engineering, subjectNameEn=null, picCn=jxjNdnQvHSQ8b9q0zS7Bgw==, picEn=4fVBwqRFt4uCO8g42aXObg==, jcr=null, cjcr=null, exts=[JournalExt(id=1319355638048740090, language=CN, name=压力容器, nameHistory1=null, nameHistory2=null, managedBy=, sponsoredBy=, publishedBy=, editorOffice=, officeProv=null, officeCity=null, officeAddr=, officeZip=, editDirector=, officeDirector=null, officePhone=null, coverPicUrl=null, journalRemark=, submitArticleUrl=null, websiteUrl=, createdTime=1792488496553, updatedTime=1792488496553, createdBy=13701087609, updatedBy=13701087609, submissionGuidelinesUrl=, submissionAuthorUrl=https://ylrq.portal.founderss.cn, submissionEditorUrl=https://journal.ids.fzyun.cn, submissionReviewUrl=https://ylrq.portal.founderss.cn, submissionCeEditorUrl=, submissionAeEditorUrl=, option={"copyright":""}), JournalExt(id=1319355638103266043, language=EN, name=Pressure Vessel Technology, nameHistory1=null, nameHistory2=null, managedBy=, sponsoredBy=, publishedBy=, editorOffice=, officeProv=null, officeCity=null, officeAddr=, officeZip=, editDirector=, officeDirector=null, officePhone=null, coverPicUrl=null, journalRemark=, submitArticleUrl=null, websiteUrl=, createdTime=1792488496566, updatedTime=1792488496566, createdBy=13701087609, updatedBy=13701087609, submissionGuidelinesUrl=, submissionAuthorUrl=https://ylrq.portal.founderss.cn, submissionEditorUrl=https://journal.ids.fzyun.cn, submissionReviewUrl=https://ylrq.portal.founderss.cn, submissionCeEditorUrl=, submissionAeEditorUrl=, option={"copyright":""})], databaseList=null, tenantJournalId=1319355204128309394, websiteList=[Website(id=1319376331645764504, webName=null, webTitle=null, webDomain=null, webCopyrigh=null, webIpcNo=null, seoTitle=null, seoKeywords=null, seoDescription=null, tenantJournalId=null, journalId=1319355204128309394, journalNameCn=null, journalNameEn=null, grayFlag=null, tenantId=1146029695717560320, platformId=null, journalGroupId=null, journalGroupNameCn=null, journalGroupNameEn=null, type=1, domain=https://castjournals.cast.org.cn/joweb/ylrq/CN, language=CN, createTime=1792493430291, createBy=18614031015, updateTime=1792493471510, updateBy=18614031015, name=压力容器-中文, tplId=1146099689490845704, title=压力容器, delFlag=0, indexPage=/home, props=[WebsiteProps(id=1319376610952856568, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=articleTextType, value=kx, createTime=1792493496883, updateTime=1792493496883, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610923496437, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=banner, value=null, createTime=1792493496876, updateTime=1792493496876, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610969633787, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=grayFlag, value=0, createTime=1792493496887, updateTime=1792493496887, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610910913524, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=logo, value=https://castjournals.cast.org.cn/joweb/ylrq/CN/file/pic?fileId=jTQ3ULyAlxRu0s8fI4nfng==, createTime=1792493496873, updateTime=1792493496873, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610986411005, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=minRunFlag, value=0, createTime=1792493496891, updateTime=1792493496891, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610944467959, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=picServerUrl, value=https://castjournals.cast.org.cn/joweb/ylrq/CN/file/pic, createTime=1792493496881, updateTime=1792493496881, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610978022396, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=silenceFlag, value=0, createTime=1792493496889, updateTime=1792493496889, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610936079350, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=staticResourcePath, value=https://castjournals.cast.org.cn/joweb/cast_kjdb_cn_619/, createTime=1792493496879, updateTime=1792493496879, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610957050873, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=themeColor, value=null, createTime=1792493496884, updateTime=1792493496884, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376610965439482, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331645764504, code=themeStyle, value=null, createTime=1792493496886, updateTime=1792493496886, creator=18614031015, updator=18614031015)]), Website(id=1319376331893228450, webName=null, webTitle=null, webDomain=null, webCopyrigh=null, webIpcNo=null, seoTitle=null, seoKeywords=null, seoDescription=null, tenantJournalId=null, journalId=1319355204128309394, journalNameCn=null, journalNameEn=null, grayFlag=null, tenantId=1146029695717560320, platformId=null, journalGroupId=null, journalGroupNameCn=null, journalGroupNameEn=null, type=1, domain=https://castjournals.cast.org.cn/joweb/ylrq/EN, language=EN, createTime=1792493430350, createBy=18614031015, updateTime=1792493467616, updateBy=18614031015, name=压力容器-英文, tplId=1146101810881728533, title=Pressure Vessel Technology, delFlag=0, indexPage=/home, props=[WebsiteProps(id=1319376586462315499, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=articleTextType, value=kx, createTime=1792493491044, updateTime=1792493491044, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586432955368, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=banner, value=null, createTime=1792493491037, updateTime=1792493491037, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586500064238, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=grayFlag, value=0, createTime=1792493491053, updateTime=1792493491053, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586420372455, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=logo, value=https://castjournals.cast.org.cn/joweb/ylrq/EN/file/pic?fileId=jTQ3ULyAlxRu0s8fI4nfng==, createTime=1792493491034, updateTime=1792493491034, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586521035760, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=minRunFlag, value=0, createTime=1792493491058, updateTime=1792493491058, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586453926890, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=picServerUrl, value=https://castjournals.cast.org.cn/joweb/ylrq/EN/file/pic, createTime=1792493491042, updateTime=1792493491042, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586512647151, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=silenceFlag, value=0, createTime=1792493491056, updateTime=1792493491056, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586441343977, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=staticResourcePath, value=https://castjournals.cast.org.cn/joweb/cast_kjdb_en_623/, createTime=1792493491039, updateTime=1792493491039, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586474898412, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=themeColor, value=null, createTime=1792493491047, updateTime=1792493491047, creator=18614031015, updator=18614031015), WebsiteProps(id=1319376586487481325, tenantId=1146029695717560320, journalId=null, journalGroupId=null, siteId=1319376331893228450, code=themeStyle, value=null, createTime=1792493491050, updateTime=1792493491050, creator=18614031015, updator=18614031015)])], journalTitle=压力容器, weixinUrl=null, journalUrl=https://www.pvtjournal.com/, iacademicId=null, status=1, seqNo=null, journalTitleEn=Pressure Vessel Technology, journalPhotoCn=jxjNdnQvHSQ8b9q0zS7Bgw==, journalPhotoEn=4fVBwqRFt4uCO8g42aXObg==, journalFirstLetter=Y, journalRecommend=null, journalNew=null, journalCollection=null, jcrJf=null, cjcrJf=null, jcrJfStr=null, cjcrJfStr=null, submissionFirstDecision=null, sciSubjectClassification=null, casSubjectClassification=null, citeScore=null, totalCitationFrequency=null, icpCode=null, psCode=null, advertisingLicenseCode=null, copyrightInformation=null, country=null, option=, provinceCode=null, provinceName=null, collectFlag=false, interPubPlatform=, interPubPlatformUrl=null), detailUrlCn=https://castjournals.cast.org.cn/joweb/ylrq/CN/10.3969/j.issn.1001-4837.2025.10.002, detailUrlEn=https://castjournals.cast.org.cn/joweb/ylrq/EN/10.3969/j.issn.1001-4837.2025.10.002, pdfUrlCn=https://castjournals.cast.org.cn/joweb/ylrq/CN/PDF/10.3969/j.issn.1001-4837.2025.10.002, pdfUrlEn=https://castjournals.cast.org.cn/joweb/ylrq/EN/PDF/10.3969/j.issn.1001-4837.2025.10.002, aliStartDate=0, aliEndDate=0, collectionFlag=false, citedCount=null, citedUrl=null, previewStatus=0, delFlag=0, hasFullText=1, orderTime=1761753600000, fullTextJson=null, articleText=null, reference=null)
收藏切换
道间温度对镍基690焊丝熔敷金属组织及性能影响研究
冯伟 1 , 孟涵 1, 2 , 韩兴海 1 , 陈波 1 , 王国佛 1
压力容器 | 试验研究 2025,42(10): 23-30
收起
收藏切换
压力容器 |试验研究 2025 , 42 (10) : 23 -30
道间温度对镍基690焊丝熔敷金属组织及性能影响研究
全屏
[Author(id=1327335691261948129, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, orderNo=0, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=Fengwei323412@163.com, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335691324862691, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335691261948129, language=EN, stringName=Wei FENG, firstName=Wei, middleName=null, lastName=FENG, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335691391971556, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335691261948129, language=CN, stringName=冯伟, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060, bio={"content":"

冯伟(1981),男,正高级工程师,主要从事特种焊接材料研发工作,通信地址:150060黑龙江省哈尔滨市平房区渤海路21号哈尔滨威尔焊接有限责任公司,E-mail:。

"}, bioImg=null, bioContent=

冯伟(1981),男,正高级工程师,主要从事特种焊接材料研发工作,通信地址:150060黑龙江省哈尔滨市平房区渤海路21号哈尔滨威尔焊接有限责任公司,E-mail:。

, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335691077398746, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, xref=1, ext=[AuthorCompanyExt(id=1327335691094175963, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China), AuthorCompanyExt(id=1327335691102564572, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060)])]), Author(id=1327335691450691814, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, orderNo=1, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335691551355113, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335691450691814, language=EN, stringName=Han MENG, firstName=Han, middleName=null, lastName=MENG, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, 2, address=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China
2Harbin Welding Institute Limited Company,Harbin 150028,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335691618463978, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335691450691814, language=CN, stringName=孟涵, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, 2, address=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060
2中国机械总院集团哈尔滨焊接研究所有限公司,哈尔滨 150028, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335691077398746, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, xref=1, ext=[AuthorCompanyExt(id=1327335691094175963, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China), AuthorCompanyExt(id=1327335691102564572, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060)]), AuthorCompany(id=1327335691161284829, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, xref=2, ext=[AuthorCompanyExt(id=1327335691182256350, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691161284829, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=2Harbin Welding Institute Limited Company,Harbin 150028,China), AuthorCompanyExt(id=1327335691190644959, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691161284829, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=2中国机械总院集团哈尔滨焊接研究所有限公司,哈尔滨 150028)])]), Author(id=1327335691681378540, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, orderNo=2, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335691752681710, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335691681378540, language=EN, stringName=Xinghai HAN, firstName=Xinghai, middleName=null, lastName=HAN, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335691832373487, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335691681378540, language=CN, stringName=韩兴海, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335691077398746, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, xref=1, ext=[AuthorCompanyExt(id=1327335691094175963, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China), AuthorCompanyExt(id=1327335691102564572, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060)])]), Author(id=1327335691912065265, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, orderNo=3, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335692004339955, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335691912065265, language=EN, stringName=Bo CHEN, firstName=Bo, middleName=null, lastName=CHEN, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335692105003252, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335691912065265, language=CN, stringName=陈波, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335691077398746, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, xref=1, ext=[AuthorCompanyExt(id=1327335691094175963, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China), AuthorCompanyExt(id=1327335691102564572, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060)])]), Author(id=1327335692167917814, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, orderNo=4, firstName=null, middleName=null, lastName=null, nameCn=null, orcid=null, stid=null, country=null, authorPic=null, dead=0, email=null, emailSecond=null, emailThird=null, correspondingAuthor=0, authorType=1, ext={EN=AuthorExt(id=1327335692289552632, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335692167917814, language=EN, stringName=Guofo WANG, firstName=Guofo, middleName=null, lastName=WANG, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null), CN=AuthorExt(id=1327335692360855801, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, authorId=1327335692167917814, language=CN, stringName=王国佛, firstName=null, middleName=null, lastName=null, prefix=null, suffix=null, authorComment=null, nameInitials=null, affiliation=null, department=null, xref=1, address=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060, bio=null, bioImg=null, bioContent=null, aboutCorrespAuthor=null)}, companyList=[AuthorCompany(id=1327335691077398746, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, xref=1, ext=[AuthorCompanyExt(id=1327335691094175963, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=EN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1Harbin Well Welding Co.,Ltd.,Harbin 150060,China), AuthorCompanyExt(id=1327335691102564572, tenantId=1146029695717560320, journalId=1319355204128309394, articleId=1327335687604515004, companyId=1327335691077398746, language=CN, country=null, province=null, city=null, postcode=null, companyName=null, departmentName=null, remark=1哈尔滨威尔焊接有限责任公司,哈尔滨 150060)])])]
冯伟1 , 孟涵1, 2, 韩兴海1, 陈波1, 王国佛1
作者信息
  • 1哈尔滨威尔焊接有限责任公司,哈尔滨 150060
  • 2中国机械总院集团哈尔滨焊接研究所有限公司,哈尔滨 150028
作者简介:

冯伟(1981),男,正高级工程师,主要从事特种焊接材料研发工作,通信地址:150060黑龙江省哈尔滨市平房区渤海路21号哈尔滨威尔焊接有限责任公司,E-mail:。

Study on the influence of interpass temperature on microstructure and properties of nickel‑based 690 welding wire deposited metal
Wei FENG1 , Han MENG1, 2, Xinghai HAN1, Bo CHEN1, Guofo WANG1
Affiliations
  • 1Harbin Well Welding Co.,Ltd.,Harbin 150060,China
  • 2Harbin Welding Institute Limited Company,Harbin 150028,China
出版时间: 2025-10-30 doi: 10.3969/j.issn.1001-4837.2025.10.002
文章导航
收藏切换

针对核岛主设备各装置焊接过程中道间温度不统一的问题,采用TIG焊方法研究道间温度对镍基690焊丝熔敷金属组织演变及力学性能的影响规律。结合拉伸、冲击等力学性能测试,以及OM,SEM,EDS等微观组织观察,结果表明:随道间温度升高,熔敷金属的室温力学性能提升不明显,但350 ℃下的强度和塑性均有所提升;随道间温度的升高,焊缝成形系数减小,熔池流动性及焊接工艺性显著改善,高温热累积效应增强,促进了熔池流动与晶界迁移,跨焊道搭接区柱状晶的取向规整度提高;当道间温度超过225 ℃时,金相组织易产生微裂纹,通过SEM,EDS分析发现,其表现为台阶状扩展形貌,并伴有O/Si元素富集及Ti/Nb元素偏析,符合高温低塑性裂纹(DDC)的特征。研究可为核电设备焊接制定合理的道间温度工艺提供参考。

Inconel 690  /  热裂纹  /  道间温度  /  高温低塑性裂纹(DDC)

To address the issue of inconsistent interpass temperatures during welding of nuclear island main equipment components,the TIG welding method was used to study the influence of interpass temperature on the microstructure evolution and mechanical properties of nickel‑based 690 welding wire deposited metal.Combined with mechanical property tests such as tensile and impact,as well as microstructural observations using OM,SEM and EDS,the results show that as the interpass temperature increases,the room‑temperature mechanical properties of the deposited metal improve insignificantly,but both strength and plasticity at 350 ℃ are enhanced.With increasing interpass temperature,the weld formation coefficient decreases,while the fluidity of the molten pool and weldability improve significantly,and the high‑temperature heat accumulation effect intensifies,promoting molten pool flow and grain boundary migration,thereby increasing the orientation regularity of columnar grains in the overlapping zone across weld passes.When the interpass temperature exceeds 225 ℃,microcracks are prone to form in the microstructure.SEM and EDS analyses reveal that these cracks exhibit step‑like propagation morphology,accompanied by O/Si element enrichment and Ti/Nb element segregation,consistent with the characteristics of ductility‑dip cracking(DDC).This study provides a reference for establishing reasonable interpass temperature processes in nuclear power equipment welding.

Inconel 690  /  hot cracking  /  interpass temperature  /  ductility‑dip cracking(DDC)
冯伟, 孟涵, 韩兴海, 陈波, 王国佛. 道间温度对镍基690焊丝熔敷金属组织及性能影响研究. 压力容器, 2025 , 42 (10) : 23 -30 . DOI: 10.3969/j.issn.1001-4837.2025.10.002
Wei FENG, Han MENG, Xinghai HAN, Bo CHEN, Guofo WANG. Study on the influence of interpass temperature on microstructure and properties of nickel‑based 690 welding wire deposited metal[J]. Pressure Vessel Technology, 2025 , 42 (10) : 23 -30 . DOI: 10.3969/j.issn.1001-4837.2025.10.002
Inconel 690合金因其优异的抗应力腐蚀性能,被广泛应用于三代核岛主设备反应堆压力容器、蒸汽发生器等关键部件的制造[1-2]。然而,该合金液态金属流动性差,焊接过程中熔池金属黏度高、焊缝成形不良,具有较高的焊接热裂纹敏感性[3-4],严重影响焊接工艺性与焊接结构质量,制约核岛主设备的结构安全性。针对这一问题,国内外学者研究多集中于熔敷金属成分的优化,通过调整Nb,Mn,Al,Ti等合金元素含量[5-7],并严格限制S,P等杂质元素[8],有效提高了Inconel 690合金焊接材料的抗裂性,并推动了焊丝成分标准的迭代。
除元素含量外,道间温度与热输入等焊接工艺参数直接影响熔敷金属的凝固行为、微观组织与力学性能,进而影响其热裂纹敏感性[9-10]。尽管通过成分优化已显著降低了Inconel 690合金的热裂纹敏感性,但焊接参数与热裂纹之间的关联机制仍存在研究不足,导致该合金在不同焊接参数下的热裂纹行为尚难以准确预测。
道间温度作为工程应用中的关键参数,显著影响焊接热循环过程。WANG等[11]研究表明,道间温度的变化可改变550 MPa级工程钢焊缝组织中贝氏体、马氏体与粗大奥氏体的体积分数,进而调控其力学性能。然而对于镍基合金,该影响可能更具材料依赖性。PETRO等[12]研究发现,道间温度对HASTELLOY C-200及HASTELLOY B-3两种镍基合金焊缝金属性能影响较小,但会加剧根部未熔合缺陷的形成。目前,关于道间温度对Inconel 690焊丝熔敷金属组织、性能及热裂纹敏感性的影响研究仍较为缺乏。
基于工程实际需求,针对国产WHS690M焊丝焊接过程中的关键问题,通过拉伸、冲击等力学性能测试,以及OM,SEM,EDS等分析手段,系统研究道间温度对其熔敷金属微观组织及力学性能的影响规律,旨在为优化国产WHS690M焊丝的焊接工艺规范提供直接、可靠的试验依据,进而指导工程实践中的道间温度选择,提升焊接接头质量及结构可靠性。
试验采用ERNiCrFe-7A焊丝,其牌号为WHS690M,规格为⌀1.2 mm,化学成分见表1。对接试验母材选用500 mm×150 mm×20 mm的Q235钢板,加工成V型坡口,坡口角度为22.5°。为防止熔敷金属被母材稀释,预先使用该焊丝在坡口内母材表面堆焊厚度6 mm以上的隔离层,如图1所示。
采用表2所示的焊接参数,并根据工程实际情况,将道间温度梯度设置为75~121,121~177,177~225,225~275 ℃。
在焊接第一道时,将试板预热至相应试验温度后进行焊接;每完成一道后,使试板空冷至该试验温度,再继续下一道次焊接。焊接完成后,依据GB/T 3323.1—2019《焊缝无损检测 射线检测 第1部分:X和伽玛射线的胶片技术》对焊缝进行射线检测(RT),结果合格。从图1所示熔敷金属中心区通过线切割截取金相试样,经磨制、抛光、腐蚀后,采用OLYMPUS GX51型光学显微镜观察其宏观组织,并结合ZEISS EVO18型扫描电子显微镜及OXFORD INCA能谱仪进行微观形貌观察与微区成分分析。
力学性能测试依据GB/T 228.1—2021《金属材料 拉伸试验 第1部分:室温试验方法》、GB/T 228.2—2015《金属材料 拉伸试验 第2部分:高温试验方法》、GB/T 229—2020《金属材料 夏比摆锤冲击试验方法》及GB/T 232—2010《金属材料 弯曲试验方法》进行,制备焊缝金属室温拉伸、350 ℃高温拉伸、室温冲击及弯曲试件,并完成相应测试。
不同道间温度下,WHS690M熔敷金属的室温及高温力学性能数据见表3,其变化趋势如图2和图3所示。可以看出,室温下熔敷金属抗拉强度均高于600 MPa,屈服强度均高于395 MPa。随着道间温度升高,熔敷金属的室温强度与塑性虽存在一定波动,但整体差异不明显。当道间温度处于177~225 ℃时,其综合力学性能最优:抗拉强度可达625 MPa,屈服强度为412 MPa,断后伸长率达47%,表现出良好的塑性。
在350 ℃高温条件下,熔敷金属的抗拉强度与屈服强度相较于室温普遍降低。当道间温度高于121 ℃时,抗拉强度虽略有提升,但屈服强度显著下降。高温下熔敷金属的塑性与室温水平相当,且随着道间温度升高,其断后伸长率呈现稳定上升趋势。道间温度处于225~275 ℃时,抗拉强度为509 MPa,断后伸长率达47%,断面收缩率为62%,在维持良好塑性的同时具备较高强度,综合力学性能最优。综合熔敷金属的室温与350 ℃力学性能可知,道间温度在177~275 ℃范围内时,其力学性能表现较佳。
冲击试验结果如表4所示,熔敷金属室温冲击吸收能量稳定在200 J以上,表明其韧性良好。对比不同道间温度下熔敷金属的冲击吸收能量可发现,其韧性在道间温度为225~275 ℃时最优,相较于道间温度121~177 ℃下的冲击吸收能量提升13.8%。侧向弯曲试验结果同样列于表4,经渗透探伤及目视检验,所有试样均未发现裂纹。
道间温度作为影响热输入的隐性焊接工艺参数,对焊丝的焊接工艺性及焊缝成形具有一定影响,并与材料冷却行为密切相关。为研究道间温度对WHS690M焊丝工艺性的影响,分别在75~121,121~177,77~225,225~275 ℃四种试验温度下进行预热,随后以表2所示焊接参数执行单道堆焊(不摆动),所得焊道截面宏观形貌如图4所示。
采用体式显微镜分别测量各焊道截面的熔宽、熔深、余高与接触角,结果如图5所示。可以看出,随道间温度升高,余高减小,接触角增大,熔深增加,而熔宽基本稳定在9.5 mm。在道间温度75~121 ℃时,熔池表面张力较大、流动性较差,导致边缘润湿性不足,接触角与熔深均为最小,焊道呈现凸起形貌。随着道间温度升高,熔池流动性改善,润湿性增强,促使接触角增大。对比可知,当道间温度较高时,焊道铺展更充分,润湿效果更为显著。
焊道成形直接关联于液态金属在熔池中的流动状态以及凝固过程中的结晶行为,对焊缝质量控制至关重要。采用焊缝成形系数对WHS690M焊丝在不同道间温度下的焊道成形进行量化,其计算方法见式(1),所测得的焊道尺寸及计算得出的焊缝成形系数如图6所示。
φ=BH
式中:φ为焊缝成形系数;B为焊缝横截面的熔宽,mm;H为焊缝横截面的熔深,mm。
可以看出,在焊接参数相同条件下,随着道间温度由75~121 ℃升高至225~275 ℃,熔深由0.75 mm增加至1.4 mm,熔宽由9.56 mm增至9.87 mm;但道间温度为121~177 ℃时,熔宽减小至7.71 mm。根据熔深与熔宽的变化可知,道间温度对焊道摊开具有积极影响,但主要作用于熔深,对熔宽影响相对较小。因此,随道间温度升高,焊缝成形系数显著减小,即焊道形貌由浅而宽逐渐转变为深而窄,表明焊道与母材熔合增强,有效提升了焊缝质量。
图7示出不同道间温度下熔敷金属的宏观金相组织。可以看出,随着道间温度逐步提升,焊道层间距离减小,这与熔深的增加趋势一致;而各焊道熔宽差异不明显,与图6中焊缝成形系数减小的规律相符。道间温度的升高使得焊接过程中各焊道之间的间隔时间缩短,在有限时间内,下一焊道搭接区域的熔深相应增加,同时促进了熔池的铺展,导致每层焊道形态趋于薄而铺展面积增大。
对焊道截面进行研磨抛光,采用CuSO4与HCl含量比为1∶2的腐蚀液进行腐蚀并观察,其金相组织如图8所示。熔敷金属组织为以柱状晶为主的奥氏体,焊道搭接区域明显,晶粒沿垂直焊接方向生长,搭接处柱状枝晶形貌不显著。对比发现,随道间温度升高,跨搭接区生长的晶粒尺寸逐渐增大。在道间温度75~121 ℃时,搭接处出现晶粒竞争长大,晶粒生长方向较为随机;当温度处于177~225℃区间时,搭接处仍呈现竞争生长趋势,但晶粒尺寸整体更大,生长方向更为一致。
对不同道间温度下的熔敷金属微观组织进行观察,仅在道间温度225~275 ℃的熔敷金属中发现了微热裂纹,其微观组织如图9所示。可以看出,热裂纹出现于搭接焊道位置,呈沿晶扩展特征,裂纹内部不光滑,并伴随有黄色规则块状析出相。裂纹两侧晶粒尺寸存在显著差异,上方晶粒尺寸明显大于裂纹下方。
根据焊道中液态金属的凝固方向推测,上部熔池金属首先完成凝固结晶。随着熔池温度下降至固相线以下,熔敷金属进入塑性下降温度区间(ductility‑dip temperature range,DTR),见图10。
FINK等[9-10]通过程控变形裂纹试验(programmable deformation crack,PVR)发现,熔敷金属在DTR温度区间内,其塑性及延展性急剧下降,导致形成狭窄的热裂纹带,该裂纹区与塑性下降温度区间的延展性损失密切相关。LIPPOLD等[13]指出,在熔敷金属凝固过程中,由于晶界滑移作用,应变将集中于晶界交叉点处;由于DTR区的存在,当外加应变超过临界应变时,易引起晶界开裂,即形成高温失塑裂纹(ductility‑dip cracking,DDC)。
为进一步确定裂纹类型,采用机械方式打开裂纹,并对裂纹断口进行SEM分析,其内部形貌如图11所示。裂纹深度约0.6 mm,与熔敷金属基体相比,其表面更为平整;熔敷金属表面可见明显因机械取样所致的塑性断裂特征,分布有大量韧窝。在低倍率下观察,裂纹断口呈现沿焊缝柱状晶开裂的特征,断口轮廓呈台阶状起伏,未见液态薄膜状相。
对裂纹内部较为平整的台阶区域进行观察,如图12所示,该区域在高倍数下呈现相对光滑且滑移特征显著的表面,可见清晰的晶界滑移痕迹。DDC裂纹在中温段的典型失塑开裂特征为塑性沿晶开裂,形貌表现为台阶起伏,高倍观察可见光滑表面伴随晶界滑移痕迹,与上述裂纹形貌相符。因此,道间温度225~275 ℃区间出现的裂纹为DDC。
对裂纹内台阶区域中呈现滑移特征的部分进行EDS分析,分析位置如图13所示,结果如表5所示。谱图6与谱图7均对应滑移区域,分析发现O,Si,Ti,Mn,Nb元素含量显著升高,其中O与Si含量远超正常水平;但谱图7所在区域的Ti,Nb元素含量较谱图6区域有明显下降。结合现有DDC形成机理,此类裂纹的形成是由于O元素导致的氧化物含量升高,降低晶间结合能,在高温塑性下降温度区间内萌生裂纹并持续沿晶扩展所致。
(1)道间温度对WHS690M熔敷金属力学性能的影响体现出强度、塑性与韧性协同优化的特征。道间温度在177~225 ℃范围内为最佳工艺窗口,该条件下熔敷金属的强度、室温塑性及高温性能综合表现最优。
(2)道间温度升高通过热累积效应显著优化了焊接工艺性与熔敷金属质量。宏观上,道间温度的提高缩短了焊道间隔时间,促进了熔池铺展,减小了焊道层间距离,改善了单层摊开性。焊缝成形系数的降低表明熔池流动性及对母材的润湿性均得到增强。微观上,熔敷金属组织为垂直焊接方向生长的柱状晶奥氏体,但随着温度升高,跨焊道搭接区的晶粒尺寸明显粗化,且生长方向趋于一致;当道间温度较低(<121 ℃)时,搭接处晶粒生长方向较为随机;而道间温度较高(177~225 ℃)时,晶粒取向的规整度明显提升。
(3)道间温度超过225℃时,熔敷金属中出现了沿晶扩展的微裂纹,经表征分析确认为高温失塑裂纹(DDC)。该裂纹呈台阶状起伏形貌,内部未见液态薄膜但可见晶界滑移痕迹,符合DDC在高温塑性下降温度区间(DTR)内的沿晶开裂特征。裂纹区域的成分分析表明,晶界处存在O、Si元素的异常富集以及Ti、Nb等元素的偏析,导致晶间结合能降低。其形成机制为:熔敷金属冷却至DTR区间时,在晶界滑移累积的应变作用下,因O、Si富集而弱化的晶界优先开裂并沿晶界扩展。

参考文献 引证文献
排序方式:
1
SEDRIKS A J,SCHULTZ J W,CORDOVI M A.Inconel alloy 690-A new corrosion resistant material[J].Corrosion Engineering,1979,28(2):82-95.
2
ZHANG R G,CARUSO M,KISER S,et al.New 30% chromium‑containing Ni-Cr-Fe welding product provides outstanding resistance to PWSCC,ductility dip cracking (DDC) and meets all other nuclear welding requirements[C]//Corrosion 2012.Association for Materials Protection and Performance,2012:1-15.
3
KISER S D,ZHANG R,BAKER B A.A new welding material for improved resistance to ductility dip cracking[C]//International Conference on Trends in Welding Research.2009.
4
ZHANG X,LI D Z,LI Y Y,et al.Effect of Nb and Mo on the microstructure, mechanical properties and ductility-dip cracking of Ni–Cr–Fe weld metals[J].Acta Metallurgica Sinica (English Letters),2016,29(10):928-939.
5
QIN R Y,WANG H,HE G.Investigation on the microstructure and ductility‑dip cracking susceptibility of the butt weld welded with ENiCrFe-7 nickel-base alloy‑covered electrodes[J].Metallurgical and Materials Transactions A,2015,46:1227-1236.
6
MO W L,LU S P,LI D Z,et al.Effects of filler metal composition on inclusions and inclusion defects for ER NiCrFe-7 weldments[J].Journal of Materials Science & Technology,2013,29(5):458-466.
7
RAPETTI, A, TODESCHINI, P, HENDILI, S,et al.A Study of ductility dip cracking of inconel 690 welding filler metal:development of a refusion cracking test[J].Proceedings of the ASME 2017 Pressure Vessels and Piping Conference,2017:V06BT06A022.
8
霍树斌,陈佩寅,陈燕,等.核用Inconel 690焊丝TIG焊微裂纹产生机理研究[J].焊接,2012(9):31-36.
HUO S B,CHEN P Y,CHEN Y,et.al.Mechanism study on micro‑crack formation in tig welds using nuclear-grade inconel 690 filler wire[J].Welding & Joining,2012(9):31-36.
9
FINK C,ZINKE M,JÜTTNER S.An investigation of ductility‑dip cracking in the base metal heat‑affected zone of wrought nickel base alloys—Part Ⅱ:Correlation of PVR and STF results[J].Welding in the World,2016,60(5):951-961.
10
FINK C.An investigation on ductility‑dip cracking in the base metal heat‑affected zone of wrought nickel base alloys—Part Ⅰ:Metallurgical effects and cracking mechanism[J].Welding in the World,2016,60(5):939-950.
11
WANG X L,TSAI Y T,YANG J R,et al.Effect of interpass temperature on the microstructure and mechanical properties of multi‑pass weld metal in a 550‑MPa‑grade offshore engineering steel[J].Welding in the World,2017,61(6):1155-1168.
12
PETRO J S.Effect of interpass temperature on the structure and properties of multipass weldments in high performance nickel alloys[D].Colorado:Colorado State University,2011.
13
LIPPOLD J C,NISSLEY N E.Further investigations of ductility‑dip cracking in high chromium,Ni‑base filler metals[J].Welding in the World,2007,51(9/10):24-30.
2025年第42卷第10期
141
56
0
引用本文
BibTeX
文章信息
doi: 10.3969/j.issn.1001-4837.2025.10.002
  • 接收时间:2025-07-26
  • 首发时间:2026-11-11
  • 出版时间:2025-10-30
补充材料
相关文章
文章信息
作者
出版历史
  • 收稿日期:2025-07-26
  • 修回日期:2025-09-19
基金
作者信息
    1哈尔滨威尔焊接有限责任公司,哈尔滨 150060
    2中国机械总院集团哈尔滨焊接研究所有限公司,哈尔滨 150028
参考文献
分享链接
https://castjournals.cast.org.cn/joweb/ylrq/CN/10.3969/j.issn.1001-4837.2025.10.002
分享至
全文二维码

扫描看全文

引用本文
BibTeX
本文的引用情况
2种不同金属材料的力学参数
科
Family
属数
Number of
genus
种数
Number of
species
占总种数比例
Percentage of
total species (%)
属
Genus
种数
Number of
species
占总种数比例
Percentage of total
species (%)
鹅膏菌科Amanitaceae 2 11 5.26 鹅膏菌属 Amanita 10 4.78
小菇科 Mycenaceae 2 12 5.74 丝盖伞属 Inocybe 5 2.39
多孔菌科 Polyporaceae 8 14 6.70 蜡蘑属 Laccaria 5 2.39
红菇科 Russulaceae 3 23 11.00 小皮伞属 Marasmius 6 2.87
小菇属 Mycena 11 5.26
光柄菇属 Pluteus 5 2.39
红菇属 Russula 17 8.13
栓菌属 Trametes 5 2.39
关闭全屏